Preparation method of pyromellitic dianhydride

By using vanadium nitrogen-doped carbon catalyst and symmetric octahydroanthracene in the liquid phase, the by-product generation and high cost problems under high temperature oxidation conditions in the prior art are solved, and the high efficiency of phenylatic dianhydride is achieved , low-cost, environmentally friendly production.

CN115925716BActive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110973827.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-24
Publication Date
2024-11-26
Estimated Expiration
2041-08-24

AI Technical Summary

Technical Problem

The existing production methods of phenylatic acid dianhydride have problems with decarboxylation reaction and by-product generation under high-temperature oxidation conditions, and rely on high-cost raw materials, resulting in high production costs and unenvironmental processes.

Method used

The vanadium nitrogen-doped carbon catalyst is used to use air/oxygen as the oxidant in the liquid phase, and symmetric octahydroanthracene as the raw material for catalytic oxidation reaction to prepare phenylatic dianhydride. The reaction conditions are mild and the process is green and environmentally friendly.

Benefits of technology

It achieves high conversion and selective acquisition of phenylatic acid dianhydride under mild conditions, reduces production costs, and provides a new preparation route that is cheap and easy to obtain, making the process more environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115925716B_ABST
    Figure CN115925716B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of fine chemical synthesis, and in particular to a method for preparing pyromellitic dianhydride. The method comprises: using a vanadium-nitrogen-doped carbon catalyst, air / oxygen as an oxidant, and symmetrical octahydroanthracene as a raw material, and performing a catalytic oxidation reaction in an organic solvent to obtain pyromellitic dianhydride. The method for preparing pyromellitic dianhydride can use symmetrical octahydroanthracene as a raw material, and prepare pyromellitic dianhydride in a liquid phase under the action of the vanadium-nitrogen-doped carbon catalyst, and the reaction conditions are mild, the process is green and environmentally friendly, the cost is low, and pyromellitic dianhydride can be obtained with a high conversion rate and selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fine chemical synthesis, and in particular to a method for preparing pyromellitic dianhydride. Background Art

[0002] Pyromellitic anhydride (1,2,4,5-benzene tetracarboxylic anhydride, referred to as PMDA) is an important chemical raw material with a wide range of uses. Polyimide synthesized from pyromellitic anhydride and aromatic diamine is a polymer material that is resistant to high temperature, deep cold, impact, and has excellent electrical and mechanical properties. In addition, pyromellitic anhydride can also be used to manufacture high-temperature resistant electrical insulating paints, plasticizers, synthetic resin crosslinking agents, and epoxy resin curing agents. Driven by the demand of downstream industries (such as IT industry, electronics industry, automobile industry, etc.), pyromellitic anhydride has broad market prospects.

[0003] The production method of pyromellitic anhydride is closely related to the selection of raw materials. Different raw materials are used, and the process routes are also different. At present, the main methods and routes at home and abroad are as follows:

[0004] 1. Using durene as raw material. It includes the early liquid phase oxidation method and the currently commonly used air gas phase oxidation method. US5225572 discloses a composite catalyst with V2O5-TiO2 as the main component. Under the condition of 350-380°C, the optimal molar yield of pyromellitic anhydride is 60.5%. CN201010543303.X discloses that the prepared catalyst active components are composed of V2O5, TiO2 and P2O5, which are loaded on SiC or porcelain rings. The catalyst has the advantages of low energy consumption and high selectivity. The process of producing pyromellitic anhydride by the gas phase oxidation method of durene is simple and can be produced continuously, but in actual production, the gas phase oxidation method of durene usually needs to be carried out under harsh high-temperature oxidation conditions, which is very easy to cause decarboxylation reaction and transition oxidation, and will generate by-products such as trimellitic anhydride and maleic anhydride. In addition, this route depends on the supply of raw material durene, and the cost is relatively high.

[0005] 2. Use trimethylbenzene (1,2,4-trimethylbenzene) as the starting material. Trimethylbenzene is first alkylated with propylene to produce 1,2,4-trimethyl-5-propylbenzene, and then liquid or gas phase oxidation is carried out to produce pyromellitic anhydride. Another route is the trimethylbenzene / carbon monoxide carbonylation method, in which trimethylbenzene is first reacted with carbon monoxide to produce high-purity 2,4,5-trimethylbenzaldehyde, and then 2,4,5-trimethylbenzaldehyde is oxidized to produce pyromellitic anhydride. The key to this type of method is to prepare high-purity intermediates such as 1,2,4-trimethyl-5-propylbenzene or 2,4,5-trimethylbenzaldehyde. However, the process route is long and the product yield is low.

[0006] Pyromellitic anhydride has a special symmetrical structure and has four carboxylic acid groups in the molecule. The raw materials have an important impact on the production cost of pyromellitic anhydride. In addition to continuing to optimize the process of the above route, developing new starting materials and fundamentally changing the production method of pyromellitic anhydride is also an important idea. Developing cheap and easily available raw materials, using mild reaction conditions, and green and environmentally friendly processes can reduce the development cost and have important application value for the green production of pyromellitic anhydride. Summary of the invention

[0007] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and provide a method for preparing pyromellitic dianhydride. The method for preparing pyromellitic dianhydride can use symmetrical octahydroanthracene as a raw material, and prepare pyromellitic dianhydride in a liquid phase under the action of a vanadium-nitrogen-doped carbon catalyst. The reaction conditions are mild, the process is green and environmentally friendly, the cost is low, and pyromellitic dianhydride can be obtained with a high conversion rate and selectivity.

[0008] In order to achieve the above object, the present invention provides a method for preparing pyromellitic anhydride, which comprises: using a vanadium-nitrogen-doped carbon catalyst, air / oxygen as an oxidant, and symmetrical octahydroanthracene as a raw material, and performing a catalytic oxidation reaction in an organic solvent to obtain pyromellitic anhydride.

[0009] The present invention can achieve the following beneficial effects:

[0010] 1. The preparation method of pyromellitic dianhydride provided by the present invention uses symmetrical octahydroanthracene as raw material. Symmetrical octahydroanthracene can be obtained by selective hydrogenation of anthracene, and anthracene is an important component of coal tar, so octahydroanthracene can be obtained from cheap coal tar, further reducing the production cost of pyromellitic dianhydride. Compared with the traditional method relying on durene and trimethylolbenzene, the present invention provides a new preparation route.

[0011] 2. The catalyst provided by the present invention is cheap and readily available, and can help reduce the production cost of pyromellitic dianhydride.

[0012] 3. The catalyst provided by the present invention can be used to prepare pyromellitic anhydride in the liquid phase using environmentally friendly molecular oxygen as an oxidant. Compared with the high-temperature gas-phase oxidation method used in the traditional technical route, the reaction conditions are milder, environmentally friendly, and have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 is the XRD pattern of the catalyst prepared in Preparation Example 1. DETAILED DESCRIPTION

[0014] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0015] In a first aspect, the present invention provides a method for preparing pyromellitic anhydride, the method comprising: using a vanadium-nitrogen-doped carbon catalyst, air / oxygen as an oxidant, and symmetrical octahydroanthracene as a raw material, and performing a catalytic oxidation reaction in an organic solvent to obtain pyromellitic anhydride.

[0016] According to the present invention, in order to obtain pyromellitic dianhydride with higher conversion rate and selectivity, the amount of the catalyst used is 0.5-30wt% (for example, it can be 0.5wt%, 1wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt% and a value within the range formed by any two of the above values) relative to symmetrical octahydroanthracene, and more preferably 1-5wt%.

[0017] According to the present invention, preferably, relative to symmetrical octahydroanthracene, the amount of the organic solvent used is 200-2000wt% (for example, it can be 200wt%, 500wt%, 800wt%, 1000wt%, 1300wt%, 1500wt%, 1800wt%, 2000wt% and a value within the range formed by any two of the above values), more preferably 500-1100wt%.

[0018] According to the present invention, preferably, the organic solvent is selected from at least one of methanol, acetic acid, methyl acetate, ethyl acetate, dichloromethane, acetonitrile, propionitrile, isobutyronitrile, dimethyl sulfoxide and acetone, more preferably at least one of acetic acid and ethyl acetate.

[0019] According to the present invention, in order to obtain pyromellitic dianhydride with higher conversion rate and selectivity, preferably, the temperature of the catalytic oxidation reaction is 60-180°C (for example, it can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C and a value within the range formed by any two of the above values), more preferably 100-160°C.

[0020] According to the present invention, in order to obtain pyromellitic dianhydride with higher conversion rate and selectivity, preferably, the catalytic oxidation reaction time is 4-18h (for example, it can be 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 18h and a value within the range formed by any two of the above values), more preferably 8-15h.

[0021] According to the present invention, in order to obtain pyromellitic dianhydride with higher conversion rate and selectivity, preferably, the partial pressure of oxygen in the oxidant is 0.01-2MPa (for example, it can be 0.01MPa, 0.1MPa, 0.3MPa, 0.5MPa, 0.8MPa, 1MPa, 1.3MPa, 1.5MPa, 1.8MPa, 2MPa and a value within the range formed by any two of the above values), more preferably 0.1-1MPa.

[0022] According to the present invention, in order to obtain pyromellitic dianhydride with higher conversion rate and selectivity, preferably, in the reaction process, the consumed oxygen is supplemented. The amount of the supplemented oxygen is such that the partial pressure of oxygen is close to the oxygen partial pressure at the beginning of the reaction. The closeness refers to 0.8-1.3 times the oxygen partial pressure at the beginning of the reaction.

[0023] According to the present invention, preferably, symmetrical octahydroanthracene, the catalyst and the solvent are added to a high-pressure reactor, and then the reactor is closed, oxygen is charged, and then the temperature is raised to the reaction temperature under stirring, and the reaction time is experienced, and during this period, the consumed oxygen is replenished. After the reaction is completed, it is cooled to room temperature and carefully reduced to normal pressure, and the reacted materials are subjected to solid-liquid separation, and the product is obtained after removing the catalyst.

[0024] According to the present invention, in order to enable the catalyst to obtain pyromellitic anhydride with higher conversion rate and selectivity, preferably, the preparation method of the vanadium-nitrogen-doped carbon catalyst comprises: calcining a nitrogen-containing carbon compound and a vanadium-containing compound to obtain the vanadium-nitrogen-doped carbon catalyst;

[0025] Wherein, the molar ratio of the nitrogen-containing carbon compound to the vanadium-containing compound is 1:0.25-4.

[0026] It can be understood that the vanadium-nitrogen doped carbon catalyst is in the form of black solid powder.

[0027] According to the present invention, in order to enable the catalyst to obtain pyromellitic anhydride with higher conversion rate and selectivity, preferably, the nitrogen-containing carbon compound is selected from at least one of o-phenanthroline, chitosan, melamine, urea, 2-picolinic acid and piperazine.

[0028] According to the present invention, in order to enable the catalyst to obtain pyromellitic dianhydride with higher conversion rate and selectivity, preferably, the vanadium-containing compound is selected from at least one of ammonium orthovanadate, ammonium metavanadate, sodium metavanadate and vanadium pentoxide.

[0029] According to the present invention, preferably, the grinding is performed at room temperature. It is understood that the nitrogen-containing carbon compound and the vanadium-containing compound are also mixed during the grinding process.

[0030] According to the present invention, in order to enable the catalyst to obtain pyromellitic dianhydride with higher conversion rate and selectivity, preferably, the calcination temperature is 500-1000°C (for example, it can be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C and a value within the range formed by any two of the above values), more preferably 600-800°C.

[0031] According to the present invention, in order to enable the catalyst to obtain pyromellitic dianhydride with higher conversion rate and selectivity, preferably, the calcination time is 0.1-20h (0.1h, 0.5h, 1h, 2h, 3h, 4h, 5h, 7h, 10h, 13h, 15h, 18h, 20h and a value within the range formed by any two of the above values), more preferably 1.5-5h.

[0032] According to the present invention, preferably, the calcination is carried out in a nitrogen environment. The nitrogen environment may be at normal pressure.

[0033] According to the present invention, preferably, after the nitrogen-containing compound and the vanadium-containing compound are fully ground and mixed, the materials are loaded into a porcelain boat and then heated to the calcination temperature at a heating rate of 6-15°C / min under the protection of nitrogen at normal pressure. After the calcination time, the temperature is gradually cooled to room temperature to obtain the vanadium-nitrogen doped carbon catalyst.

[0034] According to a particularly preferred embodiment of the present invention, symmetrical octahydroanthracene, vanadium nitrogen doped carbon catalyst and ethyl acetate are added to a high-pressure reactor, wherein the amount of the vanadium nitrogen doped carbon catalyst is 1-1.5wt% relative to 1g of symmetrical octahydroanthracene, and the amount of the ethyl acetate is 870-930wt%; after closing the reactor, 0.1-0.2MPa of oxygen is charged, the temperature is raised to 150-160°C under stirring, and the reaction is carried out for 11-13h, during which the consumed oxygen is supplemented to keep the oxygen pressure close to the oxygen partial pressure at the beginning of the reaction. After the reaction is completed, the material is cooled to room temperature, and the pressure is carefully reduced to normal pressure, and the material is filtered to obtain the pyromellitic anhydride.

[0035] The present invention will be described in detail below through examples.

[0036] Preparation Example 1

[0037] Used to illustrate the catalyst provided by the present invention and its preparation method

[0038] 10 g of melamine and 9.2 g of ammonium metavanadate (melamine: ammonium metavanadate molar ratio = 1:1) were weighed respectively, fully mixed and ground, and loaded into a porcelain boat. Under the protection of nitrogen at normal pressure, the temperature was raised to 700 ° C at a heating rate of 10 ° C / min, and then slowly cooled to room temperature after roasting for 3 hours to obtain a black solid powder, and a vanadium-nitrogen-doped carbon material catalyst A was obtained. Its XRD pattern is as follows Figure 1 shown.

[0039] Preparation Example 2

[0040] Used to illustrate the catalyst provided by the present invention and its preparation method

[0041] Weigh 10 g of piperazine and 13.4 g of ammonium metavanadate (molar ratio of piperazine: ammonium metavanadate = 1:1) respectively, mix and grind them thoroughly, load the feed into a porcelain boat, and heat the mixture to 600 ° C at a heating rate of 10 ° C / min under nitrogen protection at normal pressure. After calcining for 1.5 hours, slowly cool the mixture to room temperature to obtain a black solid powder, i.e., the vanadium-nitrogen-doped carbon material catalyst B described in the present invention.

[0042] Preparation Example 3

[0043] Used to illustrate the catalyst provided by the present invention and its preparation method

[0044] Weigh 10 g of o-phenanthroline and 6.4 g of ammonium metavanadate (o-phenanthroline: ammonium metavanadate molar ratio = 1:1) respectively, mix and grind them thoroughly, load the feed into a porcelain boat, and heat the mixture to 800 ° C at a heating rate of 10 ° C / min under the protection of nitrogen at normal pressure. After keeping the temperature for 5 hours, slowly cool it to room temperature to obtain a black solid powder, i.e., the vanadium nitrogen doped carbon material catalyst C of the present invention.

[0045] Preparation Example 4-9

[0046] Catalysts were prepared according to the method of Preparation Example 1, except that the amount of melamine used was 10 g, and the amount of ammonium metavanadate used was added according to the molar ratio of melamine to ammonium metavanadate in Table 1. The obtained catalysts were respectively recorded as Catalyst D, Catalyst E, Catalyst F, Catalyst G, Catalyst H, and Catalyst I.

[0047] Table 1

[0048] Preparation Example Molar ratio catalyst Preparation Example 4 Melamine: ammonium metavanadate = 1:4 D Preparation Example 5 Melamine: ammonium metavanadate = 1:3 E Preparation Example 6 Melamine: ammonium metavanadate = 1:2 F Preparation Example 7 Melamine: ammonium metavanadate = 1:0.5 G Preparation Example 8 Melamine: ammonium metavanadate = 1: 0.33 H Preparation Example 9 Melamine: ammonium metavanadate = 1: 0.25 I

[0049] Preparation Examples 10-15

[0050] According to Table 2, nitrogen-containing carbon compounds and vanadium compounds in different proportions were weighed, mixed and ground thoroughly, loaded into a porcelain boat, and heated to 800°C at a heating rate of 10°C / min under the protection of nitrogen at normal pressure. After keeping warm for 1.5 hours, the temperature was slowly cooled to room temperature to obtain a vanadium-nitrogen doped carbon material catalyst. The catalysts prepared in Preparation Examples 10-15 were respectively recorded as Catalyst J, Catalyst K, Catalyst L, Catalyst M, Catalyst N, and Catalyst O.

[0051] Table 2

[0052] Preparation Example Catalyst (molar ratio) catalyst Preparation Example 10 Piperazine: sodium metavanadate = 1:1 J Preparation Example 11 O-phenanthroline: vanadium pentoxide = 1:1 K Preparation Example 12 o-Phenanthroline: ammonium orthovanadate = 1:2 L Preparation Example 13 2-Pyridinecarboxylic acid: ammonium metavanadate = 1:3 M Preparation Example 14 Urea: vanadium pentoxide = 1:4 N Preparation Example 15 Chitosan: sodium metavanadate = 1:0.5 O

[0053] Example 1

[0054] Used to illustrate the method for preparing pyromellitic dianhydride provided by the present invention

[0055] Take 1g of symmetrical octahydroanthracene, 0.05g of catalyst A and about 8g of acetonitrile and add them to a 100mL high-pressure reactor. Close the reactor, fill it with 1.0MPa of oxygen, heat it to 130°C with stirring, and react for 8h. During this period, replenish the consumed oxygen to maintain the oxygen pressure at about 1.0MPa during the reaction. After the reaction is completed, cool the material to room temperature and carefully reduce the pressure to normal pressure.

[0056] Example 2

[0057] Used to illustrate the method for preparing pyromellitic dianhydride provided by the present invention

[0058] Take 1g of symmetrical octahydroanthracene, 0.01g of catalyst B and about 9g of ethyl acetate and add them into a 100mL high-pressure reactor. After closing the reactor, fill it with 0.1MPa of oxygen, heat it to 160°C with stirring, and react for 12h. During this period, replenish the consumed oxygen to maintain the oxygen pressure at about 0.1MPa during the reaction. After the reaction is completed, cool the material to room temperature and carefully reduce the pressure to normal pressure.

[0059] Example 3

[0060] Used to illustrate the method for preparing pyromellitic dianhydride provided by the present invention

[0061] Take 1g of symmetrical octahydroanthracene, 0.04g of catalyst C and about 10.5g of acetic acid and add them into a 100mL high-pressure reactor. After closing the reactor, fill it with 0.5MPa of oxygen, heat it to 100℃ with stirring, and react for 15h. During this period, replenish the consumed oxygen to maintain the oxygen pressure of about 0.5MPa during the reaction. After the reaction is completed, cool the material to room temperature and carefully reduce the pressure to normal pressure.

[0062] Embodiment 4-9

[0063] The method of Example 1 was used to prepare pyromellitic dianhydride, except that Examples 4-9 used Catalyst D, Catalyst E, Catalyst F, Catalyst G, Catalyst H, and Catalyst I prepared in Preparation Examples 4-9, respectively.

[0064] Examples 10-15

[0065] According to the following method, catalyst J, catalyst K, catalyst L, catalyst M, catalyst N and catalyst O of Preparation Examples 10-15 were used to prepare pyromellitic dianhydride.

[0066] Take 1g of symmetrical octahydroanthracene, 0.02g of catalyst, and about 5.25g of acetic acid and add them into a 100mL high-pressure reactor. After closing the reactor, fill it with 0.5MPa of oxygen, heat it to 140°C with stirring, and react for 10h. During this period, replenish the consumed oxygen to maintain the oxygen pressure at about 0.5MPa during the reaction. After the reaction is completed, cool the material to room temperature and carefully reduce the pressure to normal pressure.

[0067] Example 16

[0068] Used to illustrate the method for preparing pyromellitic dianhydride provided by the present invention

[0069] Take 1g of symmetrical octahydroanthracene, 0.005g of catalyst A and about 2g of acetonitrile and add them to a 100mL high-pressure reactor. Close the reactor, fill it with 0.01MPa of oxygen, heat it to 60°C with stirring, and react for 18h. During this period, replenish the consumed oxygen to maintain the oxygen pressure at about 0.01MPa during the reaction. After the reaction is completed, cool the material to room temperature and carefully reduce the pressure to normal pressure.

[0070] Embodiment 17

[0071] Used to illustrate the method for preparing pyromellitic dianhydride provided by the present invention

[0072] Take 1g of symmetrical octahydroanthracene, 0.3g of catalyst A and about 20g of acetonitrile and add them to a 100mL high-pressure reactor. Close the reactor, fill it with 2MPa of oxygen, heat it to 180℃ with stirring, and react for 4h. During this period, replenish the consumed oxygen to maintain the oxygen pressure at about 2MPa during the reaction. After the reaction is completed, cool the material to room temperature and carefully reduce the pressure to normal pressure.

[0073] Comparative Example 1

[0074] The method of Example 1 was used to prepare pyromellitic dianhydride, except that the vanadium nitrogen-doped carbon catalyst was replaced by the catalyst in Example 5 in CN108640926A.

[0075] Test Example 1

[0076] After the reaction of Examples 1-17 and Comparative Example 1, the catalysts were filtered out and samples were taken. The products were quantitatively analyzed by liquid chromatography to obtain the conversion rate of symmetrical octahydroanthracene and the selectivity of pyromellitic dianhydride. The results are shown in Table 3.

[0077] Table 3

[0078]

[0079]

[0080] From the results in Table 3, it can be seen that Examples 1-17 using the technical solution of the present invention have significantly better conversion rates and selectivities, among which Examples 1-15 have better conversion rates and selectivities. The conversion rate and selectivity of Comparative Example 1 are relatively poor.

[0081] In addition, the method of the present invention provides a new synthesis route of pyromellitic dianhydride, and can prepare pyromellitic dianhydride in a liquid phase, and the temperature of the catalytic oxidation reaction is 60-180° C. Compared with the prior art, the reaction conditions of the present invention are mild, the cost is low, it is green and environmentally friendly, and the process route is relatively short. Moreover, the present invention can also obtain a higher conversion rate and selectivity under milder reaction conditions.

[0082] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing pyromellitic dianhydride, characterized in that: The method comprises: using vanadium nitrogen doped carbon catalyst, air / oxygen as oxidant, symmetrical octahydroanthracene as raw material, carrying out catalytic oxidation reaction in an organic solvent to obtain pyromellitic dianhydride; The preparation method of the vanadium-nitrogen doped carbon catalyst comprises: calcining a nitrogen-containing carbon compound and a vanadium-containing compound to obtain the vanadium-nitrogen doped carbon catalyst; Wherein, the molar ratio of the nitrogen-containing carbon compound to the vanadium-containing compound is 1:0.25-4; The nitrogen-containing carbon compound is selected from at least one of o-phenanthroline, chitosan, melamine, urea, 2-picolinic acid and piperazine; The vanadium-containing compound is selected from at least one of ammonium orthovanadate, ammonium metavanadate, sodium metavanadate and vanadium pentoxide.

2. The method according to claim 1, wherein: The amount of the vanadium-nitrogen-doped carbon catalyst used is 0.5-30 wt % relative to the symmetrical octahydroanthracene.

3. The method according to claim 1 or 2, wherein: The amount of the organic solvent used is 200-2000wt% relative to the symmetrical octahydroanthracene; And / or, the organic solvent is selected from at least one of methanol, acetic acid, methyl acetate, ethyl acetate, dichloromethane, acetonitrile, propionitrile, isobutyronitrile, dimethyl sulfoxide and acetone.

4. The method according to claim 1 or 2, wherein: The temperature of the catalytic oxidation reaction is 60-180°C.

5. The method according to claim 1 or 2, wherein: The catalytic oxidation reaction time is 4-18h.

6. The method according to claim 1 or 2, wherein: The partial pressure of oxygen in the oxidant is 0.01-2 MPa.

7. The method according to claim 1, wherein: The amount of the vanadium-nitrogen-doped carbon catalyst is 1-5 wt % relative to the symmetrical octahydroanthracene; and / or, relative to the symmetrical octahydroanthracene, the amount of the organic solvent is 500-1100 wt %; And / or, the temperature of the catalytic oxidation reaction is 100-160°C; And / or, the catalytic oxidation reaction time is 8-15h; And / or, the partial pressure of oxygen in the oxidant is 0.1-1 MPa.

8. The method according to claim 1, wherein: The calcination temperature is 500-1000°C; And / or, the calcination time is 0.1-20h.

9. The method according to claim 1, wherein: The calcination temperature is 600-800°C; And / or, the calcination time is 1.5-5h.