A copper surface micro-etching and roughening liquid and its application

By adding copper ions, chloride ions, organic acids, organic acids and corrosion inhibitors to the copper surface micro-etching roughening liquid, the problem of inconsistent copper crystallization treatment effect is solved, and the improvement of copper surface roughness and dielectric materials are achieved. The enhanced adhesion is suitable for high-end PCB manufacturing, reducing the manufacturing defects of circuit boards.

CN115928072BActive Publication Date: 2024-11-08上海天承化学有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211719239.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-11-08
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

The existing copper surface etching coarse liquid is inconsistent when treating different copper crystals, and its applicability is limited, making it difficult to meet the needs of line width, line spacing reduction and density in high-end PCB manufacturing, and it is prone to seepage or oil throwing, resulting in line The board is scrapped.

Method used

The copper surface micro-etching roughening liquid containing copper ions, chloride ions, organic acids, organic acids and corrosion inhibitors is used to improve the roughness of the copper surface by adjusting the concentration and composition of solvents and solutes, and is suitable for different copper crystals. Enhance adhesion of dielectric materials and metals.

Benefits of technology

Effectively improves the roughness of the copper surface, enhances the adhesion of the photosensitive resist layer and ink, is suitable for different copper crystals, expands the scope of application, reduces the occurrence of plating and oil throwing, and improves the manufacturing of printed circuit boards. Efficiency and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115928072B_ABST
    Figure CN115928072B_ABST
Patent Text Reader

Abstract

The present invention provides a copper surface micro-etching and roughening liquid and its application, wherein the solvent of the copper surface micro-etching and roughening liquid includes water, and the solute includes copper ions, chloride ions, organic acids, organic acid salts and 0.00001-0.007 mol / L of corrosion inhibitor. The copper surface micro-etching and roughening liquid provided by the present invention can effectively improve the roughness of the copper surface, thereby improving the adhesion of dielectric materials such as photosensitive resists and inks, and metals such as tin, nickel, palladium and gold on the copper surface; on the other hand, it has better micro-etching and roughening effects on copper surfaces with different copper crystals, and has a wide range of applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of printed circuit board manufacturing, and relates to a copper surface micro-etching and roughening liquid, in particular to a copper surface micro-etching and roughening liquid and an application thereof. Background Art

[0002] With the miniaturization, lightness, thinness and functional diversification of electronic consumer products, the printed circuit board industry is driven to develop in the direction of high density, high integration, multi-layer and refinement. This trend is particularly evident for the development of high-end PCBs. As the line width and line spacing continue to shrink, the density of the line spacing continues to increase, and the processing accuracy of the traditional subtractive method cannot meet the requirements satisfactorily. At present, dense and fine circuit boards are mainly realized by the additive method, which mainly includes the following processes: drilling-glue removal-hole metallization-graphic transfer (filming-exposure-development)-electroplating-film stripping-etching-surface treatment / solder mask. Throughout the process, micro-etching and roughening of the copper surface have been carried out throughout the entire process, which is to clean the copper surface and increase the roughness of the copper surface, and improve the adhesion of other materials on the copper surface. For example, in the graphic transfer process, the copper surface needs to be micro-etched and roughened before coating the dry film to improve the adhesion of the dry film on the copper surface. If the adhesion of some films is poor, the subsequent electroplating process is prone to permeation, which leads to incomplete subsequent etching and the scrapping of the circuit board. Another example is the solder mask process. The copper surface also needs to be roughened before treatment. Otherwise, oil throwing will easily occur, requiring rework, which is time-consuming and labor-intensive.

[0003] Existing copper surface micro-etching roughening liquid can be mainly divided into two categories. The first category is the sulfuric acid hydrogen peroxide system. The roughness of the plate surface treated by this system is uniform, but it is easily contaminated by chloride ions. For example, patent CN104342701A discloses a sulfuric acid-hydrogen peroxide roughening liquid. The roughening can effectively improve the surface roughness of sputtered copper and enhance the adhesion of dry film on the sputtered copper surface by adding tetrazole compounds as corrosion inhibitors. The second category is the copper (iron) ion / organic acid system. The performance of this system is less affected by chloride ions and can form a concave and convex microstructure on the copper surface. For example, patent CN1629357 discloses an organic acid roughening agent containing a non-ionic polymer compound, which can make the copper surface obtain a certain roughness and a higher surface drop value. Patent CN103890233A discloses an organic acid super-roughening agent containing a non-ionic surfactant, which makes the metal surface concave and convex to obtain better adhesion. However, the organic acid roughening system has a strong selectivity for copper crystals, resulting in the same micro-etching roughening solution showing different roughening effects on different copper crystals. It is not generally applicable to different types of copper materials produced by different processes.

[0004] In summary, the existing micro-etching and roughening liquid still has some shortcomings, and it is still necessary to develop a new type of roughening and micro-etching liquid. Summary of the invention

[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a copper surface micro-etching and roughening liquid and its application. The copper surface micro-etching and roughening liquid provided by the present invention can, on the one hand, effectively improve the roughness of the copper surface, thereby improving the adhesion of dielectric materials such as photosensitive resist layers and inks, and metals such as tin, nickel, palladium and gold on the copper surface; on the other hand, it has better micro-etching and roughening effects on copper surfaces with different copper crystals, and has a wide range of applications.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] The invention provides a copper surface micro-etching and roughening solution, wherein the solvent of the copper surface micro-etching and roughening solution comprises water, and the solute comprises copper ions, chloride ions, organic acids, organic acid salts and 0.00001-0.007 mol / L of a corrosion inhibitor.

[0008] The copper surface micro-etching and roughening liquid provided by the present invention can, on the one hand, effectively improve the roughness of the copper surface, thereby improving the adhesion of dielectric materials such as photosensitive resists and inks, and metals such as tin, nickel, palladium and gold on the copper surface; on the other hand, it has better micro-etching and roughening effects on copper surfaces with different copper crystals, and has a wide range of applications.

[0009] The solvent of the copper surface micro-etching roughening solution in the present invention includes 0.00001 to 0.007 mol / L of corrosion inhibitor, for example, it can be 0.00001 mol / L, 0.00002 mol / L, 0.00005 mol / L, 0.0001 mol / L, 0.0002 mol / L, 0.0005 mol / L, 0.0007 mol / L, 0.001 mol / L, 0.002 mol / L, 0.005 mol / L or 0.007 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0010] In the present invention, the copper ions are provided by any one of a copper ion source, a chloride ion source or an organic acid salt or a combination of at least two thereof, and the chloride ions are provided by a copper ion source and / or a chloride ion source.

[0011] Preferably, the concentration of the copper ion is 0.3-0.6 mol / L, for example, it can be 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, 0.55 mol / L or 0.6 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0012] Preferably, the copper ions are provided by a copper ion source, and the copper ion source includes any one of copper chloride, copper formate, copper oxalate, copper acetate, copper citrate, copper diethylhexanoate or copper gluconate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of copper chloride and copper formate, a combination of copper formate and copper oxalate, a combination of copper oxalate and copper acetate, a combination of copper acetate and copper citrate, a combination of copper diethylhexanoate and copper gluconate, a combination of copper chloride, copper formate and copper oxalate, or a combination of copper acetate, copper citrate, copper diethylhexanoate and copper gluconate, preferably copper chloride.

[0013] Preferably, the concentration of chloride ions is 0.7-1.4 mol / L, for example, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L or 1.4 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] Preferably, the chloride ions are provided by a chloride ion source, which includes any one of sodium chloride, potassium chloride, calcium chloride, zinc chloride, and copper chloride, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium chloride and potassium chloride, a combination of potassium chloride and calcium chloride, a combination of zinc chloride and copper chloride, a combination of sodium chloride, potassium chloride and calcium chloride, or a combination of potassium chloride, calcium chloride, zinc chloride and copper chloride, preferably sodium chloride and / or copper chloride.

[0015] Preferably, the concentration of the organic acid is 1 to 2 mol / L, for example, it can be 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L or 2 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the organic acid comprises any one of formic acid, acetic acid, citric acid, malic acid, maleic acid, acrylic acid, gluconic acid or glycine, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of formic acid and acetic acid, a combination of acetic acid and citric acid, a combination of malic acid and maleic acid, a combination of acrylic acid and gluconic acid, a combination of gluconic acid and glycine, a combination of formic acid, acetic acid and citric acid, or a combination of malic acid, maleic acid, acrylic acid and gluconic acid.

[0017] Preferably, the concentration of the organic acid salt is 1 to 2.5 mol / L, for example, it can be 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, 2 mol / L, 2.2 mol / L, 2.4 mol / L or 2.5 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the organic acid radical ion of the organic acid salt includes any one of formate ion, acetate ion, citrate ion, malate ion, maleate ion, acrylate ion, gluconate ion or glycine ion, or a combination of at least two thereof, and a typical but non-limiting combination includes a combination of formate ion and acetate ion, a combination of acetate ion and citrate ion, a combination of malate ion and maleate ion, a combination of maleate ion and acrylate ion, a combination of gluconate ion and glycine ion, or a combination of formate ion, acetate ion and citrate ion; the metal ion includes any one of sodium ion, potassium ion or copper ion, or a combination of at least two thereof, and a typical but non-limiting combination includes a combination of sodium ion and potassium ion, a combination of potassium ion and copper ion, a combination of sodium ion and copper ion, or a combination of sodium ion, potassium ion and copper ion.

[0019] Preferably, the corrosion inhibitor includes any one of diallyldimethylammonium chloride, N,N,N-3-(2-methylallylamide)-1-propylammonium chloride, methacryloyloxyethyl trimethylammonium chloride, polydiallyldimethylammonium chloride, polyquaternium-7, polyquaternium-11 or 1-butyl-3-methylimidazole tetrafluoroborate, or a combination of at least two thereof. Typical but non-limiting combinations include diallyldimethylammonium chloride and N,N,N-3-(2-methylallylamide)-1-propylammonium chloride, N,N,N-3-(2-methylallylamide)-1-propylammonium chloride, and N,N,N-3-(2-methylallylamide)-1-propylammonium chloride. -1-propylammonium chloride in combination with methacryloyloxyethyltrimethylammonium chloride, a combination of polydimethylammonium chloride and polyquaternium-7, a combination of polyquaternium-11 and 1-butyl-3-methylimidazolium tetrafluoroborate, a combination of diallyldimethylammonium chloride, N,N,N-3-(2-methylallylamido)-1-propylammonium chloride and methacryloyloxyethyltrimethylammonium chloride, or a combination of N,N,N-3-(2-methylallylamido)-1-propylammonium chloride, methacryloyloxyethyltrimethylammonium chloride, polydimethylammonium chloride and polyquaternium-7.

[0020] Preferably, the solute of the copper surface micro-etching and roughening solution also includes an additional corrosion inhibitor, and the molar concentration of the additional corrosion inhibitor is 0.00001-0.0002 mol / L, for example, it can be 0.00001 mol / L, 0.00002 mol / L, 0.00005 mol / L, 0.00007 mol / L, 0.0001 mol / L, 0.00013 mol / L, 0.00015 mol / L, 0.00017 mol / L, 0.00019 mol / L or 0.0002 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0021] Preferably, the additional corrosion inhibitor comprises an organic cationic compound.

[0022] The organic cationic compound of the present invention contains, in addition to the quaternary ammonium bond, other groups in the molecule, such as amino, imino, amide and the like, which can react with copper or copper ions.

[0023] Preferably, the solute of the copper surface micro-etching roughening solution also includes a wetting agent, and the molar concentration of the wetting agent is 0.001-0.05 mol / L, for example, it can be 0.001 mol / L, 0.003 mol / L, 0.005 mol / L, 0.007 mol / L, 0.009 mol / L, 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L or 0.05 mol / L, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the wetting agent includes any one of sodium cumene sulfonate, N-(2-hydroxyethyl)-N-(2-ethylhexyl) β-alanine monosodium salt, polyethylene glycol or isomeric decanol polyoxyethylene ether, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium cumene sulfonate and N-(2-hydroxyethyl)-N-(2-ethylhexyl) β-alanine monosodium salt, a combination of N-(2-hydroxyethyl)-N-(2-ethylhexyl) β-alanine monosodium salt and polyethylene glycol, a combination of polyethylene glycol and isomeric decanol polyoxyethylene ether, or a combination of sodium cumene sulfonate, N-(2-hydroxyethyl)-N-(2-ethylhexyl) β-alanine monosodium salt and polyethylene glycol.

[0025] Preferably, the pH value of the copper surface micro-etching and roughening solution is 2.8-3.0, for example, it can be 2.8, 2.82, 2.84, 2.86, 2.88, 2.9, 2.92, 2.94, 2.96, 2.98 or 3, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the density of the copper surface micro-etching roughening solution is 1.06-1.26 g / cm 3 , for example, it can be 1.06 g / cm 3 , 1.07g / cm 3 , 1.08g / cm 3 , 1.09g / cm 3 , 1.10g / cm 3 , 1.11g / cm 3 , 1.12g / cm 3 , 1.13g / cm 3 , 1.14g / cm 3 , 1.15g / cm 3 , 1.16g / cm 3 , 1.17g / cm 3 , 1.18g / cm 3 , 1.19g / cm 3 , 1.20g / cm 3 , 1.21g / cm 3 , 1.22g / cm 3 , 1.23g / cm 3 , 1.24g / cm 3 , 1.25g / cm 3 or 1.26 g / cm 3 , but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] In a second aspect, the present invention provides an application of the copper surface micro-etching and roughening liquid described in the first aspect, wherein the copper surface micro-etching and roughening liquid is used for manufacturing printed circuit boards.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The copper surface micro-etching and roughening liquid provided by the present invention can, on the one hand, effectively improve the roughness of the copper surface, thereby improving the adhesion of dielectric materials such as photosensitive resists and inks, and metals such as tin, nickel, palladium and gold on the copper surface; on the other hand, it has better micro-etching and roughening effects on copper surfaces with different copper crystals, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the surface SEM of the electroplated plate (current density 0.5 ASD) after the copper surface was treated with the roughening solution in Example 1.

[0031] Figure 2 This is the surface SEM of the electroplated board (current density 3ASD) after the copper surface was treated with the roughening solution in Example 1.

[0032] Figure 3This is a surface SEM of a copper clad laminate (produced by Chang Chun Group, Taiwan, China) after the copper surface was treated with a micro-etching roughening solution in Example 1.

[0033] Figure 4 This is the surface SEM of the copper clad laminate (produced by Mitsui Copper Foil (Guangdong) Co., Ltd.) after the copper surface was treated with micro-etching and roughening solution in Example 1.

[0034] Figure 5 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with the micro-etching roughening solution in Example 1.

[0035] Figure 6 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with the micro-etching roughening solution in Example 2.

[0036] Figure 7 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with the micro-etching roughening solution in Example 3.

[0037] Figure 8 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with the micro-etching roughening solution in Example 4.

[0038] Fig. 9 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with the micro-etching roughening solution in Example 5.

[0039] Fig.10 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with micro-etching and roughening solution in Example 6.

[0040] Fig.11 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with micro-etching and roughening solution in Example 7.

[0041] Fig.12 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with micro-etching and roughening solution in Example 8.

[0042] Fig.13 This is the surface SEM of the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) after the copper surface was treated with micro-etching and roughening liquid in Comparative Example 1. DETAILED DESCRIPTION

[0043] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0044] Example 1

[0045] This embodiment provides a copper surface micro-etching and roughening solution, wherein the pH value of the copper surface micro-etching and roughening solution is 2.8-3.0, and the density is 1.06-1.26 g / cm 3 , the solvent is water, and the solute includes the following molar concentration components:

[0046]

[0047] Wherein, the additional corrosion inhibitor is trimethylammonium chloride acetohydrazide.

[0048] Example 2

[0049] This embodiment provides a copper surface micro-etching and roughening solution, wherein the pH value of the copper surface micro-etching and roughening solution is 2.8-3.0, and the density is 1.06-1.26 g / cm 3 , the solvent is water, and the solute includes the following molar concentration components:

[0050]

[0051]

[0052] Wherein, the additional corrosion inhibitor is 1-(2-hydrazino-2-oxoethyl)pyridine-1-ammonium chloride.

[0053] Example 3

[0054] This embodiment provides a copper surface micro-etching and roughening solution, wherein the pH value of the copper surface micro-etching and roughening solution is 2.8-3.0, and the density is 1.06-1.26 g / cm 3 , the solvent is water, and the solute includes the following molar concentration components:

[0055]

[0056] Wherein, the additional corrosion inhibitor is N,N,N-triethyl 2-hydrazino-2-oxoethylammonium chloride.

[0057] Example 4

[0058] This embodiment provides a copper surface micro-etching and roughening solution, wherein the pH value of the copper surface micro-etching and roughening solution is 2.8-3.0, and the density is 1.06-1.26 g / cm 3 , the solvent is water, and the solute includes the following molar concentration components:

[0059]

[0060]

[0061] Wherein, the additional corrosion inhibitor is N-(3-(trimethylammonium)propyl)methacrylimide hydrochloride.

[0062] Example 5

[0063] This embodiment provides a copper surface micro-etching and roughening solution, wherein the pH value of the copper surface micro-etching and roughening solution is 2.8-3.0, and the density is 1.06-1.26 g / cm 3 , the solvent is water, and the solute includes the following molar concentration components:

[0064]

[0065] Wherein, the additional corrosion inhibitor is 3-amino-N,N,N-trimethylpropane-1-ammonium chloride hydrochloride.

[0066] Example 6

[0067] This embodiment provides a copper surface micro-etching and roughening solution, which is the same as that of Embodiment 1 except that diallyldimethylammonium chloride and 1-butyl-3-methylimidazolium tetrafluoroborate are replaced by guanidine hydrochloride.

[0068] Example 7

[0069] This embodiment provides a copper surface micro-etching and roughening solution, which is the same as that of Embodiment 1 except that the polyamine cationic compound C-1800 is replaced by polyethyleneimine.

[0070] Example 8

[0071] This embodiment provides a copper surface micro-etching and roughening solution, which is the same as that of Embodiment 1 except that the solute does not include the polyamine cationic compound C-1800.

[0072] Example 9

[0073] This embodiment provides a copper surface micro-etching and roughening solution, which is the same as that of Embodiment 1 except that the molar concentration of the polyamine cationic compound C-1800 is 0.0005 mol / L.

[0074] Comparative Example 1

[0075] This comparative example provides a copper surface micro-etching and roughening solution, which is the same as Example 1 except that the solute does not include diallyldimethylammonium chloride and 1-butyl-3-methylimidazolium tetrafluoroborate.

[0076] Comparative Example 2

[0077] This comparative example provides a copper surface micro-etching and roughening solution, which is the same as Example 1 except that the molar concentration of diallyldimethylammonium chloride is 0.005 mol / L and the molar concentration of 1-butyl-3-methylimidazolium tetrafluoroborate is 0.007 mol / L.

[0078] To evaluate the performance of the copper surface micro-etching roughening solution, the following tests were performed:

[0079] The process of the spray test is: pickling-water washing-micro-etching-water washing-pickling-water washing-hot air drying; the temperature of the copper surface micro-etching and roughening liquid used in the spray test is 30°C, and the spray pressure is 1kg / cm 2 , the spray machine line speed is 1m / min, the effective spray length is 50cm; the pickling solution is a hydrochloric acid aqueous solution with a mass fraction of 37%wt;

[0080] 1. Micro-etching rate test

[0081] A 5 cm × 10 cm copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) was placed in a sprayer and sprayed with the copper surface micro-etching roughening solution in Examples 1 to 9 and Comparative Examples 1 and 2 for 1 min. The mass of the copper clad laminate before and after spraying was recorded. The micro-etching rate was calculated as follows: micro-etching rate (μm / min) = (m1-m2) / (2×s×ρ)×10000, where m1 and m2 are the masses of the copper clad laminate before and after spraying, respectively; ρ is the density of copper, which is 8.96 g / cm 3 ; S is the area of ​​the copper clad laminate, and the calculated micro-etching rate results are shown in Table 1.

[0082] 2. Roughness test

[0083] The copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) was roughened and micro-etched using the copper surface micro-etching roughening liquid in Examples 1 to 9 and Comparative Examples 1 and 2. The roughening amount was 1.0 μm. The surface roughness data Ra and Rz values ​​of the copper clad laminate after roughening and micro-etching were obtained by Olympus 3D measurement laser microscope (OLS5100) as shown in Table 1.

[0084] 3. Uniformity test

[0085] The copper surface micro-etching roughening solution in Examples 1 to 9 and Comparative Examples 1 and 2 was used to roughen the copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.), and the surface micromorphology of the copper clad laminate after roughening and micro-etching was measured by scanning electron microscopy, and the surface uniformity of the copper clad laminate after micro-etching was evaluated under a 2500 times scanning electron microscope image. The evaluation results of the uniformity are shown in Table 1, and the evaluation criteria are:

[0086]

[0087] 4. Dry film adhesion test

[0088] The copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) was roughened and microetched with the copper surface microetching roughening liquid in Examples 1 to 9 and Comparative Examples 1 and 2, and the roughening microetching amount was 0.7 μm; after the roughening microetching treatment, a dry film resist layer was first laminated on the surface of the copper clad laminate after the roughening microetching, and after exposure and curing treatment, 100 small grids of 1 mm×1 mm were cut on the dry film by a grid knife, and then the small grid area was completely covered with 3M tape, and peeled off in the vertical direction. By observing the small grid peeling situation, the adhesion strength of the dry film on the copper clad laminate was evaluated. The evaluation results are shown in Table 1, and the evaluation criteria are:

[0089]

[0090]

[0091] 5. Solder mask ink adhesion test

[0092] The copper clad laminate (produced by Guangzhou Taihe Circuit Board Co., Ltd.) was roughened and micro-etched with the copper surface micro-etching roughening liquid in Examples 1 to 9 and Comparative Examples 1 and 2, and the roughening amount was 1.0 μm; after the roughening and micro-etching treatment, the surface of the copper clad laminate after the roughening and micro-etching was first coated with an ink with a thickness of 25 μm, and the copper clad laminate coated with the ink was transferred to an oven, baked at 80°C for 3 hours, then exposed, and finally continued to bake at 150°C for 1 hour. After the baking was completed, two incisions with an interval of 1 cm were cut on the surface of the solder mask ink with a scalpel, and then soaked in 6N hydrochloric acid for 10 minutes, washed and dried, and then 3M600 series tape was attached to the ink surface for peeling treatment, and the adhesion strength of the solder mask ink on the copper clad laminate was evaluated. The evaluation results are shown in Table 1, and the evaluation criteria are as follows:

[0093]

[0094] 6. Morphology test

[0095] The electroplated board was subjected to micro-etching and roughening with the copper surface micro-etching and roughening solution provided in Example 1. The electroplated board used was obtained by electroplating copper in electroplating solution with a copper-clad board provided by Guangzhou Taihe Circuit Board Co., Ltd. The thickness of the copper layer deposited after electroplating was 20 μm. The current density used during the copper electroplating was 0.5 ASD (to obtain electroplated board 1) and 3 ASD (to obtain electroplated board 2), respectively. The electroplating solution was the commercial electroplating solution SkyPlate 6257 produced by Shanghai Tiancheng Chemical Co., Ltd. The SEM images of electroplated boards 1 and 2 after micro-etching and roughening treatment were respectively tested by scanning electron microscope as shown in FIG. Figure 1 and Figure 2 As shown;

[0096] The copper surface micro-etching roughening liquid provided in Example 1 was used to micro-etch and roughen the copper clad laminates produced by China Taiwan Changchun Group, Mitsui Copper Foil (Guangdong) Co., Ltd. and Guangzhou Taihe Circuit Board Co., Ltd., and the copper clad laminates after micro-etching and roughening were tested by scanning electron microscope to obtain SEM images of the copper clad laminates after micro-etching and roughening. Figure 3 , Figure 4 and Figure 5 As shown;

[0097] The copper surface micro-etching roughening liquid provided in Examples 2 to 8 and Comparative Example 1 was used to micro-etch and roughen the copper clad laminate produced by Guangzhou Taihe Circuit Board Co., Ltd., and the copper clad laminate after micro-etching and roughening was tested by scanning electron microscope to obtain SEM images of the copper clad laminate after micro-etching and roughening, as shown in FIG. Figures 6 to 13 shown.

[0098] Table 1

[0099]

[0100]

[0101] According to the data in Table 1 and Figures 1 to 13 We can get:

[0102] (1) The copper surface micro-etching roughening solution in Examples 1 to 5 is generally applicable to the micro-etching roughening of copper-clad laminates with different copper crystals. Regardless of whether the copper-clad laminates are produced by different manufacturers or electroplated at different current densities, after being roughened by the micro-etching roughening solution, the copper surface can form a concave-convex microstructure; from the perspective of roughness, the roughness Ra value of the copper-clad laminates treated with the copper surface micro-etching roughening solution in Examples 1 to 5 fluctuates in the range of 0.36 to 0.43 μm, and the Rz value fluctuates in the range of 3.02 to 3.34 μm. The copper surface micro-etching roughening solution provided by the present invention can effectively improve the roughness of the copper surface; from the perspective of uniformity, no obvious large grains are found on the surface of the copper-clad laminates treated with the copper surface micro-etching roughening solution in Examples 1 to 5, and the uniformity is all at level I; from the perspective of the adhesion strength of the dry film and the solder resist ink, the copper-clad laminates treated with the copper surface micro-etching roughening solution in Examples 1 to 5 have a high adhesion strength to the dry film and the solder resist ink, and the adhesion strength reaches level I;

[0103] (2) By comparing Example 1 with Example 6, it can be seen that the composition of the corrosion inhibitor will affect the performance of the copper surface micro-etching roughening solution. If the corrosion inhibitor is replaced with guanidine hydrochloride, the micro-etching rate will be slowed down, the uniformity of the micro-etching will be poor, and the adhesion strength of the dry film and the solder mask ink will be reduced. This is because guanidine hydrochloride has a low molecular weight and does not contain a quaternary ammonium bond in the molecule. The adsorption on the copper surface is mainly through physical adsorption, and the adsorption capacity is weak and it is easy to desorb, making it difficult for the roughening solution to effectively roughen the copper surface, resulting in a low roughness and poor roughness uniformity of the roughened copper surface, thereby reducing the adhesion strength of the dry film and the solder mask ink on the roughened copper surface;

[0104] (3) By comparing Example 1 with Example 7, it can be seen that the composition of the additional corrosion inhibitor will affect the performance of the copper surface micro-etching roughening solution. If the additional corrosion inhibitor is replaced with polyethyleneimine, the adhesion strength of the dry film and the solder mask ink will be reduced. This is because there are a large number of amino groups and imino groups in the polyethyleneimine molecule, which are easy to complex with copper ions, but difficult to directly react with elemental copper. Therefore, when the additional corrosion inhibitor is polyethyleneimine, it is more likely to be attached to the copper surface by forming a complex film with copper ions. During the spraying process, the film layer is easily broken by impact, resulting in discontinuous roughening of the copper surface during the action of the roughening micro-etching solution, resulting in an increase in the difference in the roughening effect of each point. Therefore, the overall surface roughness and roughness uniformity after roughening are worse than those of Example 1;

[0105] (4) By comparing Example 1 with Examples 8 and 9, it can be seen that the molar concentration of the additional corrosion inhibitor will affect the performance of the copper surface micro-etching roughening solution. If the additional corrosion inhibitor is not included, the micro-etching rate will be slowed down, the uniformity of the micro-etching will be poor, and the adhesion strength of the dry film and the solder mask ink will be reduced. This is because the additional corrosion inhibitor has the function of a leveling agent. Its molecules have both quaternary ammonium bonds and other active groups such as amino groups, and are highly active. It can effectively physically and chemically adsorb on the grain boundaries of copper grains, especially larger copper grains, thereby promoting corrosion, so that large copper grains can also be roughened, and the corrosion uniformity is improved. When the micro- When the etching and roughening solution does not contain an additional corrosion inhibitor, large copper grains cannot be effectively corroded and roughened, which slows down the micro-etching rate and the large copper grains cannot be effectively roughened, resulting in a decrease in the adhesion strength of the dry film and solder mask ink on the roughened copper surface; if the molar concentration of the additional corrosion inhibitor is too high, the roughness uniformity of the roughened copper surface will also deteriorate. This is because the concentration of the additional corrosion inhibitor is too high and the adsorption amount of the additional corrosion inhibitor at the grain boundary is too large, resulting in severe inhibition of corrosion at the grain boundary, resulting in local non-corrosion or less corrosion, which in turn leads to reduced roughness, poor uniformity, and reduced adhesion of the dry film and solder mask ink;

[0106] (5) By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the molar concentration of the corrosion inhibitor will affect the performance of the micro-etching roughening solution for the copper surface. If the corrosion inhibitor is not included, the micro-etching rate will slow down, the uniformity of the micro-etching will drop sharply, and the adhesion strength of the dry film and the solder mask ink will be extremely small. This is because in the absence of corrosion inhibitor, the corrosion condition of each point of the copper grain is only affected by the additional corrosion inhibitor. The concentration of the additional corrosion inhibitor is relatively low, and the effect on the overall corrosion of the copper surface is limited. Therefore, it is difficult for the copper surface to form a better roughness. If the molar concentration of the corrosion inhibitor is too high, the micro-etching rate of the micro-etching roughening solution will decrease and the roughening effect will deteriorate. This is because the corrosion inhibitor concentration is too high, and the corrosion inhibition of the overall copper grains on the copper surface is too strong, resulting in local non-corrosion or slight corrosion, which in turn causes the local roughness to be too low and the overall roughness difference becomes larger.

[0107] In summary, the copper surface micro-etching and roughening liquid provided by the present invention can, on the one hand, effectively improve the roughness of the copper surface, thereby improving the adhesion of dielectric materials such as photosensitive resists and inks, and metals such as tin, nickel, palladium and gold on the copper surface; on the other hand, it has better micro-etching and roughening effects on copper surfaces with different copper crystals, and has a wide range of applications.

[0108] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A copper surface micro-etching and roughening solution, characterized in that: The solvent of the copper surface micro-etching roughening solution includes water, and the solute includes copper ions, chloride ions, organic acids, organic acid salts and 0.00001-0.007 mol / L of corrosion inhibitor; The corrosion inhibitor includes a combination of at least two of diallyldimethylammonium chloride, N,N,N-3-(2-methylallylamido)-1-propylammonium chloride, methacryloyloxyethyltrimethylammonium chloride, polydiallyldimethylammonium chloride, polyquaternium-7, polyquaternium-11 or 1-butyl-3-methylimidazolium tetrafluoroborate; The solute of the copper surface micro-etching roughening solution also includes an additional corrosion inhibitor; the additional corrosion inhibitor is any one of trimethylammonium chloride acetohydrazide, 1-(2-hydrazino-2-oxoethyl)pyridine-1-ammonium chloride, N,N,N-triethyl-2-hydrazino-2-oxoethylammonium chloride, N-(3-(trimethylammonium)propyl)methacrylimide hydrochloride, and 3-amino-N,N,N-trimethylpropane-1-ammonium chloride hydrochloride; The molar concentration of the additional corrosion inhibitor is 0.00001-0.0002 mol / L.

2. The copper surface micro-etching and roughening solution according to claim 1, characterized in that: The concentration of the copper ions is 0.3-0.6 mol / L.

3. The copper surface micro-etching and roughening solution according to claim 2, characterized in that: The copper ions are provided by a copper ion source, and the copper ion source includes any one of copper chloride, copper formate, copper oxalate, copper acetate, copper citrate, copper diethylhexanoate or copper gluconate, or a combination of at least two thereof.

4. The copper surface micro-etching and roughening solution according to claim 3, characterized in that: The copper ion is copper chloride.

5. The copper surface micro-etching and roughening solution according to claim 1, characterized in that: The concentration of the chloride ions is 0.7-1.4 mol / L.

6. The copper surface micro-etching and roughening solution according to claim 5, characterized in that: The chloride ions are provided by a chloride ion source, and the chloride ion source includes any one of sodium chloride, potassium chloride, calcium chloride, zinc chloride, and copper chloride, or a combination of at least two of them.

7. The copper surface micro-etching and roughening solution according to claim 6, characterized in that: The chloride ions are sodium chloride and / or copper chloride.

8. The copper surface micro-etching and roughening solution according to claim 1, characterized in that: The concentration of the organic acid is 1-2 mol / L.

9. The copper surface micro-etching and roughening solution according to claim 8, characterized in that: The organic acid includes any one of formic acid, acetic acid, citric acid, malic acid, maleic acid, acrylic acid, gluconic acid or glycine, or a combination of at least two thereof.

10. The copper surface micro-etching and roughening solution according to claim 1, characterized in that: The concentration of the organic acid salt is 1-2.5 mol / L.

11. The copper surface micro-etching and roughening solution according to claim 10, characterized in that: The organic acid ions of the organic acid salt include any one of formate ion, acetate ion, citrate ion, malate ion, maleate ion, acrylate ion, gluconate ion or glycine ion, or a combination of at least two of them; the metal ions include any one of sodium ion, potassium ion or copper ion, or a combination of at least two of them.

12. The copper surface micro-etching and roughening solution according to claim 1, characterized in that: The solute of the copper surface micro-etching and roughening solution also includes a wetting agent, and the molar concentration of the wetting agent is 0.001-0.05 mol / L.

13. The copper surface micro-etching and roughening solution according to claim 12, characterized in that: The wetting agent includes any one of sodium cumene sulfonate, N-(2-hydroxyethyl)-N-(2-ethylhexyl)-β-alanine monosodium salt, polyethylene glycol or isomeric decanol polyoxyethylene ether, or a combination of at least two thereof.

14. The copper surface micro-etching and roughening solution according to claim 1, characterized in that: The pH of the copper surface micro-etching and roughening solution is 2.8-3.

0.

15. The copper surface micro-etching and roughening solution according to claim 1, characterized in that: The density of the copper surface micro-etching roughening solution is 1.06-1.26 g / cm 3 .

16. Use of the copper surface micro-etching and roughening solution according to any one of claims 1 to 15, characterized in that: The copper surface micro-etching and roughening liquid is used for manufacturing printed circuit boards.