Preparation method and application of iron-manganese-based sodium ion layered electrode material

By first preparing potassium iron-manganese base layered oxide in sodium ion battery and then performing sodium-potassium exchange, the stability and uniformity of layered oxide materials in sodium ion battery are solved, and the cycle stability and conductance of the battery are improved. It is suitable for industrial applications.

CN115947377BActive Publication Date: 2024-11-12深圳华钠新材有限责任公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310032742.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-10
Publication Date
2024-11-12
Estimated Expiration
2043-01-10

AI Technical Summary

Technical Problem

The poor structural stability and inhomogeneity of layered oxide materials in sodium ion batteries lead to poor cycle life, hindering their industrial application.

Method used

By pre-preparing the potassium iron-manganese-based layered oxide positive electrode material and exchanging sodium-potassium exchange by ion exchange method, a ferromanganese-based sodium-ion layered electrode material is obtained, thereby improving battery capacity and cycle stability.

Benefits of technology

It significantly improves the cycle stability and conductivity of the battery, improves the morphological uniformity of the material, reduces production costs, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947377B_ABST
    Figure CN115947377B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method and application of an iron-manganese-based sodium ion layered electrode material. The present invention first introduces potassium ions into the interlayer structure to increase the interlayer spacing of the transition metal oxide layer, thereby reducing resistance and enhancing conductivity, and then performs sodium-potassium exchange by an ion exchange method, so that the replaced sodium ions with small diameters are more easily deintercalated and the damage to the interlayer structure is reduced, thereby significantly improving the cycle stability. The morphology of the material obtained by the present invention is more uniform, which helps to improve the uniformity and qualified rate of industrialized products; and the preparation process is simple, does not contain expensive transition metal materials such as cobalt and nickel, and greatly reduces the production cost. The iron-manganese-based sodium ion layered electrode material obtained by the present invention has reduced resistance and significantly improved conductivity, which effectively solves the problem of low coulombic efficiency and low charge capacity of batteries prepared by using sodium-based layered oxide materials prepared by traditional high-temperature solid-phase methods or coprecipitation methods as positive electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material technology, and in particular to a preparation method and application of an iron-manganese-based sodium ion layered electrode material. Background Art

[0002] In recent years, with the further growth of social demand for energy and the general enhancement of environmental awareness, people have paid more and more attention to the development and utilization of clean and pollution-free new energy technologies, and the energy storage market has continued to expand. Among them, lithium batteries have become the leader in power batteries due to their high energy density and long cycle life. At present, they have become the dominant energy storage technology in portable electronic devices and electric vehicles. However, the shortage of lithium battery reserves, the rising cost of raw materials and the frequent occurrence of safety accidents have caused people's concerns.

[0003] Sodium-ion batteries have a similar reaction mechanism to lithium-ion batteries. They are considered to be the most promising alternatives because of their low cost, wide source of raw materials, excellent fast charging performance and good low-temperature performance. The positive electrode material is the key to its practical application. Layered oxide materials are one of the more mature technology routes currently developed. They provide large capacity and high rate capabilities due to their layered structure.

[0004] However, the capacity of sodium-ion batteries decays very quickly during application due to their poor structural stability, which has become the biggest obstacle to their practical application. The existing synthesis and preparation methods commonly used are co-precipitation method and high-temperature solid phase method, and multiple transition metal elements are doped to change the intrinsic structure of the material, but it is still difficult to avoid the problems of poor cycle life and uneven preparation process caused by the unstable structure of layered oxide materials. Improving or solving these two problems is the key to the industrialization of sodium batteries.

[0005] Existing technical means to improve the stability of sodium-based layered oxides mainly include alkali metal doping, carbon coating and core-shell structure. However, the alkali metal doping is usually in small amounts, and it is difficult to achieve material uniformity when the synthesis scale is large. Carbon coating and core-shell structure are also only suitable for the preparation of small amounts of materials, making it difficult to achieve large-scale production and single-phase uniformity of materials. Summary of the invention

[0006] The purpose of the present invention is to solve the problems of poor cycle stability and material inhomogeneity of layered oxide materials, and thus provide a method for preparing an iron-manganese-based sodium ion layered electrode material, by pre-preparing a potassium-iron-manganese-based layered oxide positive electrode material, and then performing sodium-potassium exchange by an ion exchange method, and finally obtaining an iron-manganese-based sodium ion layered electrode material, which can effectively improve the battery capacity and cycle stability.

[0007] In order to solve the above technical problems, the present invention is implemented through the following technical solutions.

[0008] The first aspect of the present invention provides a method for preparing an iron-manganese-based sodium ion layered electrode material, comprising the following steps:

[0009] (1) Fully mixing the potassium source, the iron source, and the manganese source to obtain a mixture precursor;

[0010] (2) The mixture precursor obtained in step (1) is calcined, annealed, and then cooled to room temperature to obtain a potassium iron manganese-based layered oxide positive electrode material K x Fe y Mn z O2, where 0.7<x<1.1, 0.2<y<1.0, 0<z<0.8, and y+z=1;

[0011] (3) subjecting the potassium iron manganese-based layered oxide positive electrode material in step (2) to a potassium / sodium ion exchange reaction with a sodium source;

[0012] (4) After the reaction is completed, centrifuge the precipitate, wash it and dry it to obtain an iron-manganese-based sodium ion layered electrode material, whose chemical formula is Na x Fe y Mn z O2, where 0.7<x<1.1, 0.2<y<1.0, 0<z<0.8, and y+z=1.

[0013] It should be understood that, unless otherwise specified, the x, y, z, etc. in the context of the present invention represent the relative proportion of the amount of each element. For example, when x=0.8, y=0.5, z=0.5, the chemical formula of the iron-manganese-based sodium ion layered electrode material is Na 0.8 Fe 0.5 Mn 0.5 O2, the molar ratio of Na, Fe and Mn is 0.8:0.5:0.5.

[0014] Preferably, the potassium source in step (1) is selected from one or more of potassium carbonate, potassium bicarbonate, potassium nitrate, potassium acetate, potassium hydroxide and potassium oxalate.

[0015] Preferably, the iron source in step (1) is selected from one or more of ferric oxide, ferrous oxide, ferric nitrate, ferrous nitrate and ferric carbonate.

[0016] Preferably, the manganese source in step (1) is selected from one or more of manganese dioxide, manganese tetraoxide, manganese trioxide, manganese carbonate, manganese oxalate, manganese nitrate, manganese monoxide and manganese acetate.

[0017] Preferably, in step (1), the potassium source, the iron source and the manganese source are fully mixed by ball milling.

[0018] Preferably, based on K, Fe and Mn elements, the molar ratio of potassium source, iron source and manganese source in step (1) is: 0.7-1.1: 0.2-0.99: 0.01-0.8.

[0019] Preferably, the calcination conditions in step (2) are: heating to 500-900°C at a heating rate of 3-10°C / min and calcining for 10-36h.

[0020] Preferably, the calcination in step (2) is carried out under an atmosphere of air, oxygen or argon.

[0021] Preferably, the sodium source in step (2) is selected from one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium nitrate, sodium acetate, sodium bromide, sodium iodide and sodium chloride.

[0022] Preferably, the molar ratio of sodium to potassium in the potassium / sodium ion exchange reaction in step (3) is 2-20:1.

[0023] Preferably, the potassium / sodium ion exchange reaction in step (3) is selected from one or more of a liquid phase ion exchange method and a molten salt ion exchange method.

[0024] Preferably, the liquid phase ion exchange method is as follows: the potassium iron manganese-based layered oxide positive electrode material is reacted with a sodium source and an organic solvent in a hydrothermal reactor at a low temperature and high pressure, wherein the reaction temperature is 100-240° C. and the reaction time is 1-10 h.

[0025] Preferably, the organic solvent is selected from one or more of acetonitrile and hexanol.

[0026] Preferably, the molten salt ion exchange method is as follows:

[0027] ① Calcination reaction of potassium iron manganese-based layered oxide positive electrode material and sodium source;

[0028] ② After the calcination reaction is completed, cool to room temperature, add ethanol-water mixed solution, stir evenly and then vacuum filter to remove unreacted sodium source;

[0029] ③ Dry the obtained product.

[0030] Preferably, the calcination reaction conditions in step ① are to increase the temperature to 150-400° C. at a heating rate of 3-10° C. / min and calcine for 2-6 hours.

[0031] Preferably, the calcination reaction in step ① is carried out under an atmosphere of air, oxygen or argon.

[0032] Preferably, the drying conditions in step ③ are: drying at 80° C. for 12 h.

[0033] Preferably, the centrifugation conditions in step (4) are: rotation speed 10000 rpm, centrifugation 4 times, each time 10 min.

[0034] Preferably, the washing in step (4) is performed by washing with ethanol and deionized water in sequence.

[0035] Preferably, the drying conditions in step (4) are: drying in a blast box, the drying temperature is 80° C., and the drying time is 12 h.

[0036] The second aspect of the present invention provides an iron-manganese-based sodium ion layered electrode material prepared according to the above preparation method.

[0037] The third aspect of the present invention provides a positive electrode material, comprising the above-mentioned iron-manganese-based sodium ion layered electrode material, carbon nanotubes (CNT), conductive carbon black (Super P), polyvinylidene fluoride (PVDF), and N-methylpyrrolidone (NMP).

[0038] Preferably, the positive electrode material comprises the following components in parts by weight: 80-120 parts of iron-manganese-based sodium ion layered electrode material, 5-15 parts of carbon nanotubes (CNT), 10-15 parts of conductive carbon black (Super P), 10-15 parts of polyvinylidene fluoride (PVDF), 200-300 parts of N-methylpyrrolidone (NMP). Most preferably, the positive electrode material comprises the following components in parts by weight: 100 parts of iron-manganese-based sodium ion layered electrode material, 10 parts of carbon nanotubes (CNT), 12.5 parts of conductive carbon black (Super P), 12.5 parts of polyvinylidene fluoride (PVDF), 237.5 parts of N-methylpyrrolidone (NMP).

[0039] A fourth aspect of the present invention provides a method for preparing the above-mentioned positive electrode material, comprising the following steps:

[0040] (1) Stir and disperse NMP and PVDF evenly to prepare a bonding slurry;

[0041] (2) Add CNT to the adhesive slurry and stir to disperse evenly; add Super P and stir to disperse evenly, then stop the machine and scrape the edges, then continue stirring to disperse;

[0042] (3) Adding iron-manganese-based sodium ion layered electrode material, stirring at a low speed and then increasing the stirring speed to eliminate bubbles in a vacuum environment;

[0043] (4) Stop the machine and scrape the edges, stir under vacuum high-speed stirring conditions, check the slurry viscosity, then stir at a low speed and sieve the slurry to obtain the main material;

[0044] (5) The main material prepared in step (4) is coated on the current collector and the solvent is dried.

[0045] Preferably, the stirring and dispersing in step (1) is performed at a rotation speed of 700 rpm and for 30 minutes.

[0046] Preferably, in step (2), the speed of stirring and dispersing CNT is 700 rpm for 30 min; the speed of stirring and dispersing Super P is 700 rpm for 10 min; and the speed of stirring and dispersing after stopping the machine for scraping the edges is 700 rpm for 50 min.

[0047] Preferably, the low-speed stirring in step (3) is performed at a speed of 1900 rpm for 5 min; the stirring speed after increasing is 2000 rpm for 10 min.

[0048] Preferably, in step (4), the rotation speed of the high-speed stirring is 2000 rpm, and the time is 1 hour; the rotation speed of the low-speed stirring is 700 rpm, and the time is 15 minutes; and the sieve size used for the sieving is 200 mesh.

[0049] Preferably, the current collector in step (5) is selected from aluminum foil.

[0050] A fifth aspect of the present invention provides an electrochemical device, comprising the above-mentioned positive electrode material, a separator, a negative electrode material and an electrolyte.

[0051] Preferably, the negative electrode material is selected from hard carbon negative electrode sheets.

[0052] Preferably, the electrochemical device is selected from one or more of an aluminum-plastic film soft package, a square aluminum shell, and a cylindrical steel shell.

[0053] Preferably, the electrochemical device is prepared by the following method: a positive electrode material, a separator and a negative electrode material are combined to form a core and then an electrolyte is added.

[0054] Through extensive research, the present invention has found that the preparation of iron-manganese-based sodium ion layered oxide positive electrode materials by potassium / sodium substitution can effectively solve the problems of low capacity and poor cycle stability of traditional sodium-based layered oxides. The diameter of potassium ions is larger than that of sodium. x Fe y Mn z In the process of O2 precursor, the interlayer spacing of the transition metal oxide layer is larger due to the support of potassium ions, and then Na x Fe y Mn zIn O2 materials, sodium ions replace the original positions of potassium ions, but the interlayer spacing has not been reduced, which makes the resistance to sodium ion insertion and extraction smaller, reduces resistance and thus improves conductivity. In addition, compared with the layered oxide materials prepared by conventional methods, this method reduces the resistance to sodium ion migration in and out, which reduces the damage to the interlayer structure each time sodium ions are extracted and extracted, thereby improving the stability of the interlayer structure and improving the capacity retention of the battery during long cycles. At the same time, due to the improvement of the conductivity of the material, sodium ion charging, discharging and extraction are easier, so the first cycle coulomb efficiency is improved. In addition, characterization found that the morphological uniformity of the material has been improved to a certain extent, indicating that the qualified rate of products obtained by applying this technology to industrial production is guaranteed. At the same time, the positive electrode material does not contain expensive transition metal materials such as cobalt and nickel, which greatly reduces the material cost and preparation cost of the positive electrode material, and is a potential positive electrode material for sodium ion batteries.

[0055] Compared with the prior art, the present invention has the following beneficial effects:

[0056] (1) The present invention first introduces potassium ions into the interlayer structure to increase the interlayer spacing of the transition metal oxide layer, thereby reducing resistance and enhancing conductivity. Subsequently, sodium-potassium exchange is performed by an ion exchange method, so that the replaced sodium ions with a small diameter are more easily deintercalated and the damage to the interlayer structure is reduced, thereby significantly improving the cycle stability.

[0057] (2) The present invention adopts the method of sodium / potassium ion replacement to prepare iron-manganese-based sodium ion layered electrode materials. The morphology of the obtained material is more uniform, which helps to improve the uniformity and qualified rate of industrialized products. In addition, the preparation process is simple and does not contain expensive transition metal materials such as cobalt and nickel, thereby greatly reducing the production cost.

[0058] (3) The iron-manganese-based sodium ion layered electrode material obtained by the present invention has reduced resistance and significantly improved conductivity, which effectively solves the problem of low coulombic efficiency and low specific charge capacity of batteries prepared by using sodium-based layered oxide materials prepared by traditional high-temperature solid-phase method or coprecipitation method as positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 The potassium iron manganese-based layered oxide positive electrode material KFe in Example 1 0.5 Mn 0.5 Scanning electron microscope image of O2.

[0060] Figure 2 The iron-manganese-based sodium ion layered electrode material NaFe in Example 1 0.5 Mn 0.5 Scanning electron microscope image of O2.

[0061] Figure 3This is a schematic diagram of the button battery capacity test results of Example 1.

[0062] Figure 4 This is a schematic diagram of the test results of the remaining capacity of the button-type battery in Example 1 after 1000 cycles. DETAILED DESCRIPTION

[0063] In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0064] Example 1

[0065] An iron-manganese-based sodium ion layered electrode material, the preparation method of which comprises the following steps:

[0066] (1) 0.2 mol of potassium carbonate, 0.2 mol of ferrous oxide, and 0.1 mol of manganese trioxide were placed in a planetary ball mill and ball-milled at a speed of 700 rpm for 30 min to obtain a mixture precursor;

[0067] (2) The mixture precursor obtained in step (1) is placed in a muffle furnace and heated to 700°C at a heating rate of 5°C / min and calcined for 12 hours. After annealing, it is cooled to room temperature to obtain a potassium iron manganese-based layered oxide positive electrode material KFe 0.5 Mn 0.5 O2, its scanning electron micrograph is as follows Figure 1 As shown, it can be seen that the potassium iron manganese-based layered oxide positive electrode material KFe 0.5 Mn 0.5 O2 is a micron-scale single crystal structure;

[0068] (3) Dissolve 1 mol of sodium hydroxide in 60 mL of hexanol solution and add the potassium iron manganese-based layered oxide positive electrode material KFe prepared in step (2) 0.5 Mn 0.5 O2, magnetic stirring at room temperature for 60 min, the obtained solution was placed in a hydrothermal reactor for reaction, the reaction temperature was 180 ° C, and the reaction time was 8 h;

[0069] (4) After the reaction, the mixture was centrifuged at 10,000 rpm for 4 times, each time for 10 min. The precipitate was washed with ethanol and deionized water, respectively, and then dried in a forced air drying oven at 80°C for 12 h. Thus, an iron-manganese-based sodium ion layered electrode material was obtained, whose chemical formula is NaFe 0.5 Mn 0.5 O2, its scanning electron micrograph is as follows Figure 2 shown.

[0070] Subsequently, the iron-manganese-based sodium ion layered electrode material prepared above is used to prepare a positive electrode sheet, which includes the following steps:

[0071] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 2375g of N-methylpyrrolidone, stir it under vacuum at 700rpm for 30min, and let it stand to obtain a 5% adhesive slurry; the amount of PVDF added after baking is 125g.

[0072] (2) 125 g of conductive carbon black (SuperP) and 100 g of CNT that had been pre-baked at 120 °C under vacuum conditions for 12 h were added to the adhesive slurry. After vacuum stirring at 700 rpm for 2 h, 1000 g of iron-manganese-based sodium ion layered electrode material that had been pre-baked at 120 °C under vacuum conditions for 12 h was added. Vacuum stirring at 700 rpm was continued for 2 h, and then an appropriate amount of NMP was added to adjust the viscosity to 5000 mPa·s.

[0073] (3) The main material prepared in step (2) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet with a diameter of 13 mm is obtained.

[0074] Furthermore, the composite positive electrode sheet obtained above is used to prepare a CR2032 button battery, comprising the following steps:

[0075] The composite positive electrode sheet, negative electrode sheet, electrolyte and diaphragm prepared above were assembled into a CR2032 button battery in a glove box filled with argon. The negative electrode sheet was a metal sodium sheet. The solvent of the electrolyte consisted of dimethyl carbonate, diethyl carbonate and ethyl carbonate, and the volume ratio of the three was 1:1:1. The solute of the electrolyte was 1M NaPF6, and the diaphragm model was Celgard2400.

[0076] The obtained CR2032 button battery was subjected to charge and discharge tests, with a potential range of 1.5V-4V and a test capacity of 139mAh / g ( Figure 3 ), 89% capacity remaining after 1000 cycles ( Figure 4 ).

[0077] Example 2

[0078] An iron-manganese-based sodium ion layered electrode material, the preparation method of which comprises the following steps:

[0079] (1) 0.2 mol of potassium carbonate, 0.2 mol of ferrous oxide, and 0.1 mol of manganese trioxide were placed in a planetary ball mill and ball-milled at a speed of 700 rpm for 30 min to obtain a mixture precursor;

[0080] (2) The mixture precursor obtained in step (1) is placed in a muffle furnace and heated to 700°C at a heating rate of 5°C / min and calcined for 12 hours. After annealing, it is cooled to room temperature to obtain a potassium iron manganese-based layered oxide positive electrode material KFe 0.5 Mn 0.5 O2;

[0081] (3) The potassium iron manganese-based layered oxide positive electrode material KFe in step (2) 0.5 Mn 0.5 O2 and 0.5 mol sodium nitrate were mixed evenly in a mortar, and the mixture was placed in a tube furnace with an argon atmosphere, heated to 260°C at a heating rate of 5°C / min for 4 hours, and then cooled to room temperature; 100 mL of ethanol-water mixed solution was added, stirred evenly, and unreacted sodium nitrate was removed by vacuum filtration, and the resulting product was then placed in a vacuum drying oven at 80°C for 12 hours to obtain the iron-manganese-based sodium ion layered electrode material NaFe 0.5 Mn 0.5 O2.

[0082] Subsequently, the iron-manganese-based sodium ion layered electrode material prepared above is used to prepare a positive electrode material, including the following steps:

[0083] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 2375g of N-methylpyrrolidone, stir it under vacuum at 700rpm for 30min, and let it stand to obtain a 5% adhesive slurry; the amount of PVDF added after baking is 125g.

[0084] (2) 125 g of conductive carbon black (SuperP) and 100 g of CNT that had been pre-baked at 120 °C under vacuum conditions for 12 h were added to the adhesive slurry. After vacuum stirring at 700 rpm for 2 h, 1000 g of iron-manganese-based sodium ion layered electrode material that had been pre-baked at 120 °C under vacuum conditions for 12 h was added. Vacuum stirring at 700 rpm was continued for 2 h, and then an appropriate amount of NMP was added to adjust the viscosity to 5000 mPa·s.

[0085] (3) The main material prepared in step (2) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet with a diameter of 13 mm is obtained.

[0086] Furthermore, the composite positive electrode sheet obtained above is used to prepare a CR2032 button battery, comprising the following steps:

[0087] The composite positive electrode sheet, negative electrode sheet, electrolyte and diaphragm prepared above were assembled into a CR2032 button battery in a glove box filled with argon. The negative electrode sheet was a metal sodium sheet. The solvent of the electrolyte consisted of dimethyl carbonate, diethyl carbonate and ethyl carbonate, and the volume ratio of the three was 1:1:1. The solute of the electrolyte was 1M NaPF6, and the diaphragm model was Celgard2400.

[0088] The obtained CR2032 button battery was subjected to charge and discharge tests with a potential range of 1.5V-4V and a test capacity of 150mAh / g. After 1000 cycles, 92% of the capacity remained.

[0089] Comparative Example 1

[0090] An iron-manganese-based sodium ion layered electrode material, the preparation method of which comprises the following steps:

[0091] (1) 0.2 mol of sodium carbonate, 0.2 mol of ferrous oxide, and 0.1 mol of manganese trioxide were placed in a planetary ball mill and ball-milled at a speed of 700 rpm for 30 min to fully mix them to obtain a mixture precursor;

[0092] (2) The mixture precursor obtained in step (1) is placed in a muffle furnace and heated to 700°C at a heating rate of 5°C / min and calcined for 12 hours. After annealing, it is cooled to room temperature to obtain an iron-manganese-based sodium ion layered electrode material NaFe 0.5 Mn 0.5 O2.

[0093] Subsequently, the iron-manganese-based sodium ion layered electrode material prepared above is used to prepare a positive electrode material, including the following steps:

[0094] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 2375g of N-methylpyrrolidone, stir it under vacuum at 700rpm for 30min, and let it stand to obtain a 5% adhesive slurry; the amount of PVDF added after baking is 125g.

[0095] (2) 125 g of conductive carbon black (SuperP) and 100 g of CNT that had been pre-baked at 120 °C under vacuum conditions for 12 h were added to the adhesive slurry. After vacuum stirring at 700 rpm for 2 h, 1000 g of iron-manganese-based sodium ion layered electrode material that had been pre-baked at 120 °C under vacuum conditions for 12 h was added. Vacuum stirring at 700 rpm was continued for 2 h, and then an appropriate amount of NMP was added to adjust the viscosity to 5000 mPa·s.

[0096] (3) The main material prepared in step (2) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet with a diameter of 13 mm is obtained.

[0097] Furthermore, the composite positive electrode sheet obtained above is used to prepare a CR2032 button battery, comprising the following steps:

[0098] The composite positive electrode sheet, negative electrode sheet, electrolyte and diaphragm prepared above were assembled into a CR2032 button battery in a glove box filled with argon. The negative electrode sheet was a metal sodium sheet. The solvent of the electrolyte consisted of dimethyl carbonate, diethyl carbonate and ethyl carbonate, and the volume ratio of the three was 1:1:1. The solute of the electrolyte was 1M NaPF6, and the diaphragm model was Celgard2400.

[0099] The obtained CR2032 button battery was subjected to charge and discharge tests with a potential range of 1.5V-4V and a test capacity of 132mAh / g. After 1000 cycles, 73% of the capacity remained.

[0100] Comparative Example 2

[0101] A manganese-based sodium ion layered electrode material, the preparation method of which comprises the following steps:

[0102] (1) 0.2 mol potassium carbonate and 0.1 mol manganese trioxide were placed in a planetary ball mill and ball-milled at a speed of 700 rpm for 30 min to obtain a mixture precursor;

[0103] (2) The mixture precursor obtained in step (1) is placed in a muffle furnace and heated to 700°C at a heating rate of 5°C / min and calcined for 12 hours. After annealing, it is cooled to room temperature to obtain a potassium iron manganese-based layered oxide positive electrode material KMn 0.5 O2;

[0104] (3) Dissolve 1 mol of sodium hydroxide in 60 mL of hexanol solution and add the potassium iron manganese-based layered oxide positive electrode material KMn prepared in step (2) 0.5 O2, magnetic stirring at room temperature for 60 min, the obtained solution was placed in a hydrothermal reactor for reaction, the reaction temperature was 180 ° C, and the reaction time was 8 h;

[0105] (4) After the reaction, centrifuge at 10000 rpm for 4 times, each time for 10 min. The precipitate after centrifugation is washed with ethanol and deionized water respectively, and then placed in a blast drying oven for drying at a temperature of 80 ° C and a drying time of 12 h to obtain a manganese-based sodium ion layered electrode material, whose chemical formula is NaMn 0.5 O2.

[0106] Subsequently, the manganese-based sodium ion layered electrode material prepared above is used to prepare a positive electrode sheet, which includes the following steps:

[0107] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 2375g of N-methylpyrrolidone, stir it under vacuum at 700rpm for 30min, and let it stand to obtain a 5% adhesive slurry; the amount of PVDF added after baking is 125g.

[0108] (2) Add 125 g of conductive carbon black (SuperP) and 100 g of CNT that had been pre-baked at 120 °C under vacuum conditions for 12 h to the adhesive slurry. After vacuum stirring at 700 rpm for 2 h, add 1000 g of manganese-based sodium ion layered electrode material that had been pre-baked at 120 °C under vacuum conditions for 12 h. Continue vacuum stirring at 700 rpm for 2 h, and then add an appropriate amount of NMP to adjust the viscosity to 5000 mPa·s.

[0109] (3) The main material prepared in step (2) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet with a diameter of 13 mm is obtained.

[0110] Furthermore, the composite positive electrode sheet obtained above is used to prepare a CR2032 button battery, comprising the following steps:

[0111] The composite positive electrode sheet, negative electrode sheet, electrolyte and diaphragm prepared above were assembled into a CR2032 button battery in a glove box filled with argon. The negative electrode sheet was a metal sodium sheet. The solvent of the electrolyte consisted of dimethyl carbonate, diethyl carbonate and ethyl carbonate, and the volume ratio of the three was 1:1:1. The solute of the electrolyte was 1M NaPF6, and the diaphragm model was Celgard2400.

[0112] The obtained CR2032 button battery was subjected to charge and discharge tests with a potential range of 1.5V-4V and a test capacity of 142mAh / g. After 1000 cycles, 70% of the capacity remained.

[0113] From the above, it can be seen that the sodium-based layered oxide material prepared by conventional methods such as high-temperature solid-phase method has a poor battery capacity and unsatisfactory cycle performance when used as a positive electrode material. After the potassium-iron-manganese-based layered oxide positive electrode material is first prepared by the method of the present invention, the sodium-potassium ions are exchanged by liquid phase ion exchange method or molten salt ion exchange method, and the iron-manganese-based sodium ion layered electrode material finally prepared improves the shortcomings of poor material stability from a structural perspective, enhances the cycle stability of charge and discharge, improves the coulomb efficiency of the first cycle charge and discharge, and improves the microscopic uniformity of the material, which helps to improve the qualified rate of industrialized products. While the manganese-based sodium ion layered oxide prepared by the ion replacement method after removing the iron source can improve the electrode capacity to a certain extent, its cycle capacity retention decreases rapidly and is not suitable for industrial production.

[0114] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.

Claims

1. A method for preparing an iron-manganese-based sodium ion layered electrode material, characterized in that: The steps include: (1) Fully mixing the potassium source, the iron source, and the manganese source to obtain a mixture precursor; (2) The mixture precursor obtained in step (1) is calcined, annealed, and then cooled to room temperature to obtain a potassium iron manganese-based layered oxide positive electrode material K x Fe y Mn z O2, where 0.7<x<1.1, 0.2<y<1.0, 0<z<0.8, and y+z=1; (3) subjecting the potassium iron manganese-based layered oxide positive electrode material in step (2) to a potassium / sodium ion exchange reaction with a sodium source; the potassium / sodium ion exchange reaction is selected from one or more of a liquid phase ion exchange method and a molten salt ion exchange method; The liquid phase ion exchange method is specifically as follows: the potassium iron manganese-based layered oxide positive electrode material is subjected to a low temperature and high pressure reaction with a sodium source and an organic solvent in a hydrothermal reactor, wherein the reaction temperature is 100-240° C. and the reaction time is 1-10 hours; The molten salt ion exchange method is specifically as follows: ① Calcination reaction of potassium iron manganese-based layered oxide positive electrode material and sodium source; ② After the calcination reaction is completed, cool to room temperature, add ethanol-water mixed solution, stir evenly and then vacuum filter to remove unreacted sodium source; ③ Drying the obtained product; (4) After the reaction is completed, centrifuge the precipitate, wash it and dry it to obtain an iron-manganese-based sodium ion layered electrode material, whose chemical formula is Na x Fe y Mn z O2, where 0.7<x<1.1, 0.2<y<1.0, 0<z<0.8, and y+z=1.

2. The preparation method according to claim 1, characterized in that: The potassium source in step (1) is selected from one or more of potassium carbonate, potassium bicarbonate, potassium nitrate, potassium acetate, potassium hydroxide and potassium oxalate.

3. The preparation method according to claim 1, characterized in that: The iron source in step (1) is selected from one or more of ferric oxide, ferrous oxide, ferric nitrate, ferrous nitrate and ferric carbonate.

4. The preparation method according to claim 1, characterized in that: The manganese source in step (1) is selected from one or more of manganese dioxide, manganese tetraoxide, manganese trioxide, manganese carbonate, manganese oxalate, manganese nitrate, manganese monoxide and manganese acetate.

5. The preparation method according to claim 1, characterized in that: The sodium source in step (2) is selected from one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium nitrate, sodium acetate, sodium bromide, sodium iodide and sodium chloride.

6. An iron-manganese-based sodium ion layered electrode material prepared according to the preparation method according to any one of claims 1 to 5.

7. A positive electrode material, characterized in that: The invention comprises an iron-manganese-based sodium ion layered electrode material prepared according to the preparation method according to any one of claims 1 to 5, CNT, Super P, PVDF and NMP.