Porous carbon network modified silicon dioxide composite negative electrode material and its preparation and application
By growing a porous carbon network on the surface of silicon oxide and using in-situ reduction of nickel oxide catalyst, the problem of low specific capacity and safety hazards of graphite anode materials in lithium-ion batteries is solved, and the cycle stability and conductivity of silicon oxide anode are improved. , meeting the needs of high energy density and reliability.
Patent Information
- Application Number
- CN202211696451.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-28
AI Technical Summary
The existing graphite anode material for lithium-ion batteries has a low theoretical specific capacity and is prone to produce lithium dendrites, which poses safety risks and cannot meet the needs of high energy density and high operational reliability.
In-situ reduction of nickel oxide is used as a catalyst, and a porous carbon network is grown on the surface of silicon oxide through plasma chemical vapor deposition to alleviate the volume expansion of the SiOx material during the charge and discharge process and promote the formation of a stable solid electrolyte interface layer on the surface.
It significantly improves the cycle stability and electronic conductivity of silicon oxide anode materials, alleviates the problems of volume change and poor conductivity, and improves electrochemical performance.
Smart Images

Figure CN115959671B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries and relates to a porous carbon network modified silicon oxide composite negative electrode material and a preparation method and application thereof. Background Art
[0002] Compared with other rechargeable batteries, lithium-ion batteries have higher energy density and operating voltage, lower self-discharge and maintenance requirements, and are widely used in various electronic devices and electric vehicles. However, the currently commercialized graphite anode has a low theoretical specific capacity (372 mAh g -1 ), and also because of its low working potential, it is easy to produce lithium dendrites, which has serious safety hazards and cannot meet the urgent needs of portable electronic devices and electric vehicles for high energy density and high operating reliability.
[0003] Si(SiO x )-based materials are considered to be the most promising new materials to replace traditional graphite negative electrodes due to their abundant natural resources, high specific capacity and suitable lithium insertion potential. Compared with Si materials, SiO x The material helps to establish a stable solid electrolyte interface (SEI) layer due to the in-situ formation of inert lithium oxide (Li2O) and lithium silicate (Li4SiO4) during the alloying process. x The negative electrode has a large volume change (about 200%) and poor electronic conductivity (about 6.7×10 -4 s cm -1 ) and other inherent disadvantages, resulting in poor electrochemical performance. To solve the above problems, the present invention proposes an in-situ reduction of nickel oxide as a catalyst, using plasma chemical vapor deposition (PECVD) to grow a porous carbon network on the surface of silicon oxide to alleviate SiO x The volume expansion of the material during the charging and discharging process promotes the formation of a stable SEI film on the surface, significantly improving the cycle stability of silicon monoxide negative electrode materials. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a porous carbon network modified silicon oxide composite negative electrode material by in-situ reduction of nickel oxide as a catalyst and plasma chemical vapor deposition (PECVD). The material has the advantages of high conductivity, high specific surface area, etc., and at the same time alleviates the SiO x Volume effect of materials in lithium battery applications.
[0005] To achieve the above-mentioned purpose of the invention, the technical solution of the present invention is as follows:
[0006] A method for preparing a porous carbon network modified silicon oxide composite negative electrode material, wherein the composite negative electrode material is a carbon coating with a three-dimensional network structure attached to the surface of silicon oxide particles, and the preparation method comprises the following steps:
[0007] Step 1: Pretreatment of silicon oxide powder: disperse silicon oxide powder in 1 mol / L KOH solution, stir at room temperature for 4 hours, and then wash with deionized water until neutral to obtain silicon oxide powder with rough surface;
[0008] Step 2: dispersing the silicon oxide powder obtained in step 1 in deionized water, and adding a mixed solution of nickel acetate and ammonium persulfate;
[0009] Step 3: dissolving a certain amount of ammonia solution in deionized water and diluting it 100 times, then slowly dropping the diluted ammonia solution into the mixed solution obtained in step 2, stirring at room temperature for 30 minutes after the dropping is completed, washing with deionized water until neutral, and then drying in an oven at 80° C. for 12 hours to obtain silicon dioxide powder with basic nickel oxide attached to the surface;
[0010] Step 4: The silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 is placed in a tube furnace, and a layer of carbon layer with a porous network structure is grown in situ by plasma enhanced chemical vapor deposition to form a silicon oxide composite material encapsulated by a porous network structure carbon coating. The specific process is: the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 is placed in a porcelain boat, and then placed in a tube furnace, and then heated to 350° C. in an inert atmosphere to convert the basic nickel oxide into nickel oxide, and then inert gas and reducing gas are introduced and kept warm for 60 min, reducing nickel oxide to nickel element; continuing to heat to 800-1000°C in the mixed gas atmosphere, and introducing carbon source gas and carrier gas to keep the gas pressure in the tube furnace between 100 and 110 Pa, then turning on the inductively coupled plasma RF power supply, the power output power is 300 W, the carbon growth time is 30 min, after the reaction is completed, turning off the inductively coupled plasma RF power supply, stopping the introduction of carbon source gas and carrier gas, and cooling to room temperature in an argon atmosphere to obtain a three-dimensional network structure of carbon coating encapsulated silicon oxide composite negative electrode material.
[0011] As a preferred embodiment, silicon 2 oxide powder with a particle size of 1-10 μm is used in step 1.
[0012] As a preferred embodiment, the inert gas in step 4 is any one of argon, helium and neon, with a flow rate of 200 sccm, and the reducing gas is hydrogen, which plays a role in reducing nickel oxide, with a flow rate of 20 sccm.
[0013] As a preferred embodiment, the carbon source gas in step 4 is one or a mixture of methane, ethane and acetylene, with a flow rate of 20 sccm, and the carrier gas is hydrogen, which assists the ionization of the carbon source gas, with a flow rate of 10 sccm.
[0014] As a preferred embodiment, the heating rate from room temperature to 350°C in step 4 is 2°C / min, and the temperature is kept at 350°C for 60 minutes, and then reducing gas hydrogen is introduced to reduce the nickel oxide.
[0015] As a preferred embodiment, in step 4, the heating rate from 350°C to 800-1000°C is 5°C / min, and the temperature is kept at 800-1000°C for 20 minutes before the carbon source gas is introduced.
[0016] As a preferred embodiment, in step 2, the mass ratio of nickel acetate to silicon oxide is 1:2, and the mass ratio of ammonium persulfate to silicon oxide is 1:20.
[0017] As a preferred embodiment, in step 3, an ammonia solution with an initial concentration of 28%-37% is used, wherein the molar ratio of the ammonia solution to nickel acetate is 2:1.
[0018] The present invention also provides a porous carbon network modified silicon iodide composite negative electrode material obtained by the preparation method.
[0019] The present invention also provides an application of the porous carbon network modified silicon monoxide composite negative electrode material in the preparation of a secondary battery.
[0020] The beneficial effects of the present invention are as follows: the nickel catalyst is synthesized by a solvent method, which is safe and reliable, has high repeatability, low raw material price, and is environmentally friendly. Moreover, since the metal nickel catalyst prepared by the present invention is obtained by reducing nickel oxide with hydrogen, under the catalytic action of metal nickel, a three-dimensional network-structured carbon coating can be rapidly grown on the surface of silicon oxide by plasma enhanced chemical vapor deposition. The carbon coating with a porous network structure improves the electrical contact between the active material particles at the microscopic level, which is beneficial to improving the electronic conductivity of silicon oxide, and improves the solid-liquid interface contact at the macroscopic level, which is beneficial to promoting the rapid transfer of charge. In addition, the three-dimensional porous structure can effectively release the internal stress generated by silicon oxide during the lithiation / delithiation process, and alleviate the volume swelling during the cycle. Therefore, the composite material has excellent structural stability and cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope (SEM) image of the porous carbon network modified silicon dioxide composite negative electrode material prepared in Example 1 of the method of the present invention.
[0022] Figure 2This is the cycle curve of the porous carbon network modified silicon dioxide composite negative electrode material prepared in Example 1 of the method of the present invention at a current density of 1 A / g. DETAILED DESCRIPTION
[0023] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0024] The embodiment provides a method for preparing a porous carbon network modified silicon oxide composite negative electrode material, wherein the composite negative electrode material is a carbon coating with a three-dimensional network structure attached to the surface of silicon oxide particles, and the preparation method comprises the following steps:
[0025] Step 1: Pretreatment of silicon oxide powder: disperse silicon oxide powder in 1 mol / L KOH solution, stir at room temperature for 4 hours, and then wash with deionized water until neutral to obtain silicon oxide powder with rough surface;
[0026] Step 2: dispersing the silicon oxide powder obtained in step 1 in deionized water, and adding a mixed solution of nickel acetate and ammonium persulfate;
[0027] Step 3: dissolving a certain amount of ammonia solution in deionized water and diluting it 100 times, then slowly dropping the diluted ammonia solution into the mixed solution obtained in step 2, stirring at room temperature for 30 minutes after the dropping is completed, washing with deionized water until neutral, and then drying in an oven at 80° C. for 12 hours to obtain silicon dioxide powder with basic nickel oxide attached to the surface;
[0028] Step 4: The silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 is placed in a tube furnace, and a layer of carbon layer with a porous network structure is grown in situ by plasma enhanced chemical vapor deposition to form a silicon oxide composite material encapsulated by a porous network structure carbon coating. The specific process is: the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 is placed in a porcelain boat, and then placed in a tube furnace, and then heated to 350° C. in an inert atmosphere to convert the basic nickel oxide into nickel oxide, and then inert gas and reducing gas are introduced and kept warm for 60 min, reducing nickel oxide to nickel element; continuing to heat to 800-1000°C in the mixed gas atmosphere, and introducing carbon source gas and carrier gas to keep the gas pressure in the tube furnace between 100 and 110 Pa, then turning on the inductively coupled plasma RF power supply, the power output power is 300 W, the carbon growth time is 30 min, after the reaction is completed, turning off the inductively coupled plasma RF power supply, stopping the introduction of carbon source gas and carrier gas, and cooling to room temperature in an argon atmosphere to obtain a three-dimensional network structure of carbon coating encapsulated silicon oxide composite negative electrode material.
[0029] In some embodiments, silicon 2 oxide powder with a particle size of 1-10 μm is used in step 1.
[0030] In some embodiments, the inert gas in step 4 is any one of argon, helium and neon, with a flow rate of 200 sccm, and the reducing gas is hydrogen, which plays a role in reducing nickel oxide, with a flow rate of 20 sccm.
[0031] In some embodiments, the carbon source gas in step 4 is one or a mixture of methane, ethane and acetylene, with a flow rate of 20 sccm, and the carrier gas is hydrogen, which assists in ionizing the carbon source gas, with a flow rate of 10 sccm.
[0032] In some embodiments, the heating rate from room temperature to 350° C. in step 4 is 2° C. / min, and the temperature is kept at 350° C. for 60 minutes, and then reducing gas hydrogen is introduced to reduce nickel oxide.
[0033] In some embodiments, the heating rate from 350°C to 800-1000°C in step 4 is 5°C / min, and the temperature is kept at 800-1000°C for 20 minutes before the carbon source gas is introduced.
[0034] In some embodiments, in step 2, the mass ratio of nickel acetate to silicon oxide is 1:2, and the mass ratio of ammonium persulfate to silicon oxide is 1:20.
[0035] In some embodiments, in step 3, an ammonia solution with an initial concentration of 28%-37% is used, wherein the molar ratio of the ammonia solution to nickel acetate is 2:1.
[0036] The porous carbon network modified silicon iodide composite negative electrode material obtained by the preparation method can be used to prepare secondary batteries.
[0037] Example 1
[0038] This embodiment provides a method for preparing a porous carbon network modified silicon oxide composite negative electrode material, wherein the composite negative electrode material is a carbon coating with a three-dimensional network structure attached to the surface of silicon oxide particles, and the preparation method comprises the following steps:
[0039] Step 1: Pretreatment of silicon oxide powder: disperse silicon oxide powder with a particle size of 1 μm in 1 mol / L KOH solution, stir at room temperature for 4 hours, and then wash with deionized water until neutral to obtain silicon oxide powder with a rough surface;
[0040] Step 2: Disperse the silicon oxide powder obtained in step 1 in deionized water, and add a mixed solution of nickel acetate and ammonium persulfate; the mass ratio of nickel acetate to silicon oxide is 1:2, and the mass ratio of ammonium persulfate to silicon oxide is 1:20.
[0041] Step 3: dissolving a certain amount of ammonia solution in deionized water and diluting it 100 times, then slowly dropping the diluted ammonia solution into the mixed solution obtained in step 2, stirring at room temperature for 30 minutes after the dropping is completed, washing with deionized water until neutral, and then drying in an oven at 80° C. for 12 hours to obtain silicon dioxide powder with basic nickel oxide attached to the surface;
[0042] Step 4: Place the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 in a tube furnace, and use plasma enhanced chemical vapor deposition to in situ grow a layer of carbon layer with a porous network structure to form a silicon oxide composite material encapsulated by a porous network structure carbon coating. The specific process is: place the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 in a porcelain boat, and put it into a tube furnace, and then heat it to 350°C at a heating rate of 2°C / min in an inert atmosphere, and keep it at 350°C for 60 minutes to convert the basic nickel oxide into nickel oxide, and then introduce inert gas and reducing gas and keep it warm. The reaction mixture was heated to 800°C at a heating rate of 5°C / min in a mixed gas atmosphere and kept at 800°C for 20 min. The carbon source gas and the carrier gas were then introduced to keep the gas pressure in the tube furnace between 100 and 110 Pa. The inductively coupled plasma RF power supply was then turned on with an output power of 300 W and a carbon growth time of 30 min. After the reaction was completed, the inductively coupled plasma RF power supply was turned off, and the introduction of the carbon source gas and the carrier gas was stopped. After cooling to room temperature in an argon atmosphere, a silicon oxide composite negative electrode material encapsulated in a three-dimensional network structure was obtained.
[0043] The inert gas in step 4 is argon with a flow rate of 200 sccm, and the reducing gas is hydrogen with a flow rate of 20 sccm.
[0044] The carbon source gas in step 4 is methane with a flow rate of 20 sccm, and the carrier gas is hydrogen with a flow rate of 10 sccm.
[0045] like Figure 1 Shown is a scanning electron microscope (SEM) image of the porous carbon network modified silicon oxide composite negative electrode material prepared in Example 1, which shows that the carbon layers on the surface are cross-connected with each other, presenting a porous network structure, which provides abundant channels for electron transport and ion diffusion. At the same time, the three-dimensional porous structure suppresses the volume expansion of silicon oxide to a certain extent.
[0046] The porous carbon network modified silicon oxide composite negative electrode material is prepared into an electrode sheet, and the prepared electrode sheet is assembled into a battery in a glove box, and its electrochemical performance is tested. The steps for preparing the electrode sheet are as follows: the silicon oxide material is mixed with a conductive agent and a binder in a mass ratio of 8:1:1 to prepare a slurry, and then the slurry is coated on the rough side of the copper foil, and the electrode sheet is prepared at 80°C in a vacuum oven for 12 hours. The conductive agent includes any one or more of conductive carbon black, Ketjen black, carbon nanotubes, and conductive graphite. In this embodiment, conductive carbon black is selected. The binder includes one or more of sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), sodium alginate (SA), and polyacrylic acid (PAA). In this embodiment, sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) are selected. The prepared electrode was cut into small discs with a diameter of 10 mm and placed in a glove box with oxygen and water content below 0.01 ppm; a mixed solution obtained by dissolving 1.2 M LiPF6 in a mixed solution of EC:DEC:FEC with a volume ratio of 3:6:1 and 2% VC as additives using Celgard-2500 as a separator was used as an electrolyte, and a lithium sheet was used as a counter electrode to assemble a CR2032 button battery in the glove box.
[0047] like Figure 2 The figure shows the cycle performance curve of the porous carbon network modified silicon oxide composite negative electrode material prepared in Example 1 of the method of the present invention at a current density of 1A / g. It can be observed that the porous carbon network modified silicon oxide composite negative electrode material has an initial discharge specific capacity of 2620.1mAh / g, an initial charge specific capacity of 1896.4mAh / g and an initial coulombic efficiency of 72.38%, and a discharge reversible capacity of 377mAh / g after 300 cycles, and a capacity retention rate of 57.22%.
[0048] Example 2
[0049] This embodiment provides a method for preparing a porous carbon network modified silicon oxide composite negative electrode material, wherein the composite negative electrode material is a carbon coating with a three-dimensional network structure attached to the surface of silicon oxide particles, and the preparation method comprises the following steps:
[0050] Step 1: Pretreatment of silicon oxide powder: disperse silicon oxide powder with a particle size of 10 μm in 1 mol / L KOH solution, stir at room temperature for 4 hours, and then wash with deionized water until neutral to obtain silicon oxide powder with a rough surface;
[0051] Step 2: Disperse the silicon oxide powder obtained in step 1 in deionized water, and add a mixed solution of nickel acetate and ammonium persulfate; the mass ratio of nickel acetate to silicon oxide is 1:2, and the mass ratio of ammonium persulfate to silicon oxide is 1:20.
[0052] Step 3: dissolving a certain amount of ammonia solution in deionized water and diluting it 100 times, then slowly dropping the diluted ammonia solution into the mixed solution obtained in step 2, stirring at room temperature for 30 minutes after the dropping is completed, washing with deionized water until neutral, and then drying in an oven at 80° C. for 12 hours to obtain silicon dioxide powder with basic nickel oxide attached to the surface;
[0053] Step 4: The silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 is placed in a tube furnace, and a layer of carbon layer with a porous network structure is grown in situ by plasma enhanced chemical vapor deposition to form a silicon oxide composite material encapsulated by a porous network structure carbon coating. The specific process is: the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 is placed in a porcelain boat, and then placed in a tube furnace, and then heated to 350°C at a heating rate of 2°C / min in an inert atmosphere, and kept at 350°C for 60 minutes to convert the basic nickel oxide into nickel oxide, and then inert gas and reducing gas are introduced and kept for 6 0min, reduce the nickel oxide to nickel element; continue to heat to 1000℃ at a heating rate of 5℃ / min in the mixed gas atmosphere, and keep it at 1000℃ for 20min, then introduce carbon source gas and carrier gas to keep the gas pressure in the tube furnace between 100 and 110Pa, then turn on the inductively coupled plasma RF power supply, the power output power is 300W, and the carbon growth time is 30min. After the reaction is completed, turn off the inductively coupled plasma RF power supply, stop introducing the carbon source gas and carrier gas, and cool to room temperature in an argon atmosphere to obtain a three-dimensional network structure of carbon coating encapsulated silicon oxide composite negative electrode material.
[0054] The inert gas in step 4 is helium with a flow rate of 200 sccm, and the reducing gas is hydrogen with a flow rate of 20 sccm.
[0055] The carbon source gas in step 4 is ethane with a flow rate of 20 sccm, and the carrier gas is hydrogen with a flow rate of 10 sccm.
[0056] The preparation process of the electrode sheet, the assembly and testing process of the button cell are the same as those in Example 1.
[0057] Example 3
[0058] This embodiment provides a method for preparing a porous carbon network modified silicon oxide composite negative electrode material, wherein the composite negative electrode material is a carbon coating with a three-dimensional network structure attached to the surface of silicon oxide particles, and the preparation method comprises the following steps:
[0059] Step 1: Pretreatment of silicon oxide powder: disperse silicon oxide powder with a particle size of 1-10 μm in 1 mol / L KOH solution, stir at room temperature for 4 hours, and then wash with deionized water until neutral to obtain silicon oxide powder with a rough surface;
[0060] Step 2: Disperse the silicon oxide powder obtained in step 1 in deionized water, and add a mixed solution of nickel acetate and ammonium persulfate; the mass ratio of nickel acetate to silicon oxide is 1:2, and the mass ratio of ammonium persulfate to silicon oxide is 1:20.
[0061] Step 3: dissolving a certain amount of ammonia solution in deionized water and diluting it 100 times, then slowly dropping the diluted ammonia solution into the mixed solution obtained in step 2, stirring at room temperature for 30 minutes after the dropping is completed, washing with deionized water until neutral, and then drying in an oven at 80° C. for 12 hours to obtain silicon dioxide powder with basic nickel oxide attached to the surface;
[0062] Step 4: Place the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 in a tube furnace, and use plasma enhanced chemical vapor deposition to in situ grow a layer of carbon layer with a porous network structure to form a silicon oxide composite material encapsulated by a porous network structure carbon coating. The specific process is: place the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 in a porcelain boat, and put it into a tube furnace, and then heat it to 350°C at a heating rate of 2°C / min in an inert atmosphere, and keep it at 350°C for 60 minutes to convert the basic nickel oxide into nickel oxide, and then introduce inert gas and reducing gas and keep it warm. The reaction mixture was heated to 900°C at a heating rate of 5°C / min in a mixed gas atmosphere and kept at 900°C for 20 min. The carbon source gas and the carrier gas were then introduced to keep the gas pressure in the tube furnace between 100 and 110 Pa. The inductively coupled plasma RF power supply was then turned on with an output power of 300 W and a carbon growth time of 30 min. After the reaction was completed, the inductively coupled plasma RF power supply was turned off, and the introduction of the carbon source gas and the carrier gas was stopped. After cooling to room temperature in an argon atmosphere, a silicon oxide composite negative electrode material encapsulated in a three-dimensional network structure was obtained.
[0063] The inert gas in step 4 is helium and neon with a flow rate of 200 sccm, and the reducing gas is hydrogen with a flow rate of 20 sccm.
[0064] The carbon source gas in step 4 is a mixed gas of ethane and acetylene with a flow rate of 20 sccm. The carrier gas is hydrogen with a flow rate of 10 sccm.
[0065] The preparation process of the electrode sheet, the assembly and testing process of the button cell are the same as those in Example 1.
[0066] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a porous carbon network modified silicon oxide composite negative electrode material, wherein the composite negative electrode material is a carbon coating with a three-dimensional network structure attached to the surface of silicon oxide particles. Features The preparation method comprises the following steps: Step 1: Pretreatment of silicon oxide powder: Disperse silicon oxide powder in 1 mol / L After being stirred at room temperature for 4 hours, the mixture was washed with deionized water until neutral to obtain silicon dioxide powder with a rough surface. Step 2: dispersing the silicon oxide powder obtained in step 1 in deionized water, and adding a mixed solution of nickel acetate and ammonium persulfate; Step 3: dissolving a certain amount of ammonia solution in deionized water and diluting it 100 times, then slowly dropping the diluted ammonia solution into the mixed solution obtained in step 2, stirring at room temperature for 30 minutes after the dropping is completed, washing with deionized water until neutral, and then drying in an oven at 80° C. for 12 hours to obtain silicon dioxide powder with basic nickel oxide attached to the surface; Step 4: placing the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 in a tube furnace, and using plasma enhanced chemical vapor deposition to in situ grow a carbon layer with a porous network structure to form a silicon oxide composite material encapsulated by a porous network structure carbon coating. The specific process is: placing the silicon oxide powder with basic nickel oxide attached to the surface obtained in step 3 in a porcelain boat, and putting it into a tube furnace, and then heating it to 350° C. in an inert atmosphere to convert the basic nickel oxide into nickel oxide, and then introducing an inert gas and a reducing gas and keeping the temperature for 60 minutes to reduce the nickel oxide to a single nickel substance; The mixture was then heated to 800-1000°C at a heating rate of 5°C / min in a mixed gas atmosphere, and kept at 800-1000°C for 20 minutes, and a carbon source gas and a carrier gas were introduced to keep the gas pressure in the tube furnace between 100 and 110 Pa. Subsequently, an inductively coupled plasma radio frequency power supply was turned on, and the power supply output power was 300 W. The carbon growth time was 30 minutes. After the reaction was completed, the inductively coupled plasma radio frequency power supply was turned off, and the introduction of the carbon source gas and the carrier gas was stopped. After cooling to room temperature in an argon atmosphere, a silicon oxide composite negative electrode material encapsulated in a three-dimensional network structure was obtained.
2. A method for preparing a porous carbon network modified silicon oxide composite negative electrode material according to claim 1, Features: The silicon oxide powder with a particle size of 1-10 μm is used in step 1.
3. The method for preparing a porous carbon network modified silicon oxide composite negative electrode material according to claim 1, Features: The inert gas in step 4 is any one of argon, helium and neon, with a flow rate of 200 sccm. The reducing gas is hydrogen, which plays a role in reducing nickel oxide, with a flow rate of 20 sccm.
4. The method for preparing a porous carbon network modified silicon oxide composite negative electrode material according to claim 1, Features: The carbon source gas in step 4 is one or a mixture of methane, ethane and acetylene, with a flow rate of 20 sccm. The carrier gas is hydrogen, which assists in ionizing the carbon source gas, with a flow rate of 10 sccm.
5. The method for preparing a porous carbon network modified silicon oxide composite negative electrode material according to claim 1, Features: In step 4, the heating rate from room temperature to 350° C. is 2° C. / min, and the temperature is kept at 350° C. for 60 minutes, and then reducing gas hydrogen is introduced to reduce nickel oxide.
6. The method for preparing a porous carbon network modified silicon oxide composite negative electrode material according to claim 1, Features: In the step 2, the mass ratio of nickel acetate to silicon oxide is 1:2, and the mass ratio of ammonium persulfate to silicon oxide is 1:
20.
7. The method for preparing a porous carbon network modified silicon oxide composite negative electrode material according to claim 1, Features: In step 3, an ammonia solution with an initial concentration of 28%-37% is used, wherein the molar ratio of the ammonia solution to nickel acetate is 2:
1.
8. The porous carbon network modified silicon 2 oxide composite negative electrode material obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the porous carbon network modified silicon oxide composite negative electrode material described in claim 8 in the preparation of secondary batteries.