Flower-shaped LiVPO4F material, preparation method thereof and application thereof as positive electrode material for lithium-ion batteries

Through nano-design and constructing flower-shaped LiVPO4F battery material, the problem of low conductivity of LiVPO4F in lithium-ion batteries is solved, and high specific capacity and excellent electrochemical performance are achieved to meet the needs of power lithium batteries.

CN115974044BActive Publication Date: 2024-12-06DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111205409.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-15
Publication Date
2024-12-06
Estimated Expiration
2041-10-15

AI Technical Summary

Technical Problem

The low conductivity of polyanionic LiVPO4F in lithium-ion batteries seriously restricts its actual specific capacity, rate performance and cycle stability. The existing modification methods have limited effects.

Method used

The flower-like LiVPO4F battery material is constructed through nano-design, and a three-dimensional porous morphology is formed by hydrothermal reaction, reflux and sintering, which improves the porosity and electrochemical properties of the material.

Benefits of technology

The excellent electrochemical performance of LiVPO4F material is achieved, with a specific capacity of 132.6mAh/g, meeting the needs of power lithium batteries, and improving the cycling stability and rate performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115974044B_ABST
    Figure CN115974044B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a flower-shaped LiVPO4F positive electrode material. The method comprises the following steps: dispersing vanadium pentoxide phosphoric acid in water and hydrothermally heating the material at 100-180°C for 10-24h. The hydrothermal product is added to isobutanol and refluxed at 100-150°C for 5-20h. The refluxed product is treated at 600-1000°C for 1-10h in a H2 / Ar reducing atmosphere. The reduced product is mixed with LiF and ball-milled for 1-10h. The ball-milled product is sintered at 500-100°C for 1-10h in an argon atmosphere of a tubular furnace and naturally cooled to room temperature to obtain a flower-shaped LiVPO4F. The electrode material prepared by the invention has good uniformity, high crystallinity and excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a lithium ion battery positive electrode material, and in particular to a flower-shaped LiVPO4F battery material and a preparation method thereof, belonging to the technical field of battery material preparation. Background Art

[0002] Lithium-ion batteries have been widely used as the main power source for portable electronic devices, communication tools and electric vehicles. In lithium-ion batteries, the positive electrode material plays a very important role in its performance. Lithium vanadium fluorophosphate (LiVPO4F) is a new type of polyanion positive electrode material. Its structure is a three-dimensional framework network constructed by PO4 tetrahedron and VO4F2 octahedron. In the three-dimensional structure, PO4 tetrahedron and VO4F2 octahedron share one oxygen vertex, and VO4F2 octahedron is connected by fluorine vertices. Due to its high theoretical specific capacity (156mAh g -1 ), a higher voltage platform (~4.2V) and excellent thermal stability, LiVPO4F shows great development potential. In 2003, J.Barker's research group first synthesized LiVPO4F by a solid-phase method and proved that it has good electrochemical properties. However, the electrical conductivity of the polyanion LiVPO4F is very low, which seriously restricts its actual specific capacity, rate performance and cycle stability. At present, researchers generally use bulk doping and surface coating methods to improve their battery performance, but the modification effect is still limited. On the other hand, although nanotechnology has been widely used in the preparation of other battery materials, there have been few reports on the scientific design and efficient preparation and modification of LiVPO4F using advanced and effective nanostructures. Summary of the invention

[0003] According to one aspect of the present application, a flower-shaped LiVPO4F battery material is provided, which is composed of nano-shaped primary particles self-assembled into a three-dimensional flower-like structure, forming a three-dimensional porous morphology, having good porosity, and exhibiting excellent capacity, rate and cycle performance.

[0004] The present invention provides a method for preparing a LiVPO4F material, comprising the following steps:

[0005] 1) mixing a raw material containing a vanadium source and a phosphorus source with water, and subjecting the mixture to a hydrothermal reaction to obtain an intermediate product 1; the main component of the intermediate product 1 is VOPO4·2H2O;

[0006] 2) mixing the raw material containing the intermediate product 1 and isobutanol 2, and heating the mixture for reaction to obtain a mixed solution;

[0007] 3) reflux the mixed solution at 100-150° C. for 5-20 hours to obtain a reflux product;

[0008] 4) reducing the reflux product in a reducing atmosphere to obtain an intermediate product 2, wherein the main component of the intermediate product 2 is VPO4;

[0009] 5) Mixing and ball-milling the raw materials containing the fluorine source, the lithium source and the intermediate product 2, and sintering them in an inert atmosphere to obtain the LiVPO4F material.

[0010] Optionally, the vanadium source is selected from at least one of V2O5, V2O3 or NH4VO3;

[0011] The phosphorus source is selected from at least one of NH4H2PO4, (NH4)2HPO4 or H3PO4;

[0012] The lithium source is selected from at least one of Li2CO3, LiOH or LiF;

[0013] The fluorine source is selected from at least one of LiF or NH4F;

[0014] The molar ratio of the vanadium source, phosphorus source, fluorine source and lithium source is (0.9-1.2):(0.9-1.2):(0.9-1.2):(0.9-1.2), preferably 1:1:1:1;

[0015] The molar number of the vanadium source is calculated based on the molar number of the V element in the vanadium source;

[0016] The molar number of the phosphorus source is calculated based on the molar number of the P element in the phosphorus source;

[0017] The molar number of the fluorine source is calculated based on the molar number of the F element in the fluorine source;

[0018] The molar number of the lithium source is calculated based on the molar number of the Li element in the lithium source.

[0019] Optionally, the lower limit of the molar ratio of the vanadium source, phosphorus source, fluorine source and lithium source can be independently selected from 0.8 and 0.9; the upper limit of the molar ratio of the vanadium source, phosphorus source, fluorine source and lithium source can be independently selected from 1.1 and 1.2.

[0020] Optionally, in step 1), the temperature of the hydrothermal reaction is 100 to 180° C., preferably 120 to 140° C.; the hydrothermal time is 10 to 24 hours, preferably 15 to 20 hours.

[0021] Optionally, the lower limit of the hydrothermal reaction temperature may be independently selected from 100°C, 120°C, 150°C, 160°C; the upper limit of the hydrothermal reaction temperature may be independently selected from 120°C, 150°C, 160°C, 180°C.

[0022] Optionally, the lower limit of the hydrothermal reaction time can be independently selected from 10 h, 15 h, 16 h, 20 h, and the upper limit of the hydrothermal reaction time can be independently selected from 15 h, 16 h, 20 h, and 24 h.

[0023] Optionally, in step 1), the mixing 1 is stirred at 20 to 30° C. for 30 to 100 min, preferably for 60 min, to form a dispersion.

[0024] Optionally, in step 2), the temperature of the heating reaction is 30-70° C., and the reaction time is 2-6 hours.

[0025] Optionally, the lower limit of the heating reaction temperature can be independently selected from 30°C and 50°C; the upper limit of the heating reaction temperature can be independently selected from 50°C and 70°C.

[0026] Optionally, the lower limit of the heating reaction time can be independently selected from 2h, 3h, 4h, 5h; the upper limit of the heating reaction time can be independently selected from 3h, 4h, 5h, 6h.

[0027] Optionally, in step 2), the mixing 2 is stirred at room temperature for 20 to 60 minutes to disperse the intermediate product 1 in isobutanol.

[0028] Optionally, in step 3), the reflux temperature is 100-120° C.; the reflux time is 10-15 h.

[0029] Optionally, the lower limit of the reflux temperature may be independently selected from 100°C, 110°C, 120°C; the upper limit of the reflux temperature may be independently selected from 110°C, 120°C, 150°C.

[0030] Optionally, the lower limit of the reflux time can be independently selected from 5 h, 10 h, 15 h, and the upper limit of the reflux time can be independently selected from 10 h, 15 h, and 20 h.

[0031] Optionally, in step 4), the reduction treatment is carried out at 600-1000° C. for 1-10 h; preferably 700-850° C.; preferably 2-5 h.

[0032] Optionally, the lower limit of the reduction treatment temperature may be independently selected from 600°C, 700°C, 800°C, 850°C; the upper limit of the reduction treatment temperature may be independently selected from 700°C, 800°C, 850°C, 1000°C.

[0033] Optionally, the lower limit of the reduction treatment time can be independently selected from 1 h, 2 h, and 5 h; the upper limit of the reduction treatment temperature can be independently selected from 2 h, 5 h, and 10 h.

[0034] Optionally, in step 4), the reducing atmosphere contains hydrogen, and the concentration of the hydrogen is 5-10%.

[0035] Optionally, in step 4), the reducing atmosphere contains hydrogen and an inert gas, and the inert gas is preferably argon.

[0036] Optionally, in step 5), the inert atmosphere is selected from at least one of nitrogen or argon; the ball milling speed is 100-500 rpm, preferably 300-400 h; the ball milling time is 1-10 h, preferably 4-6 h; the sintering temperature is 500-800°C, preferably 650-700°C; the sintering time is 1-10 h; preferably 2-5 h.

[0037] Optionally, the lower limit of the sintering temperature may be independently selected from 500°C, 650°C, 700°C; the upper limit of the sintering temperature may be independently selected from 650°C, 700°C, 800°C.

[0038] Optionally, the lower limit of the sintering time may be independently selected from 1 h, 2 h, and 5 h; the upper limit of the sintering time may be independently selected from 2 h, 5 h, and 10 h.

[0039] According to another aspect of the present application, a LiVPO4F material prepared by any of the above methods is provided.

[0040] Preferably, the microscopic morphology of the LiVPO4F material is a flower cluster consisting of a plurality of flowers, and each flower is composed of a plurality of stacked layers.

[0041] Preferably, the particle size of the single flower is 8-15 μm; the thickness of the nanosheet is 10-50 nm; the sheet has a porous structure; the specific surface area is 5-20 m 2 g -1 ; preferably 10m 2 g -1 ; The pore size is 2 to 5 nm.

[0042] According to another aspect of the present application, there is provided application of any of the above-mentioned LiVPO4F materials as a positive electrode material for a lithium battery.

[0043] According to another aspect of the present application, a positive electrode material for a lithium battery is provided, characterized in that the positive electrode material contains the LiVPO4F material according to any one of claims 5, 6 or 7, and the content of LiVPO4F in the positive electrode material is 50 to 90 wt%.

[0044] Optionally, the positive electrode material for lithium battery further includes components of a conductive agent and a binder; the conductive agent is preferably Ketjen black; and the binder is preferably polyvinylidene fluoride (PVDF).

[0045] The innovative features and beneficial effects of the present invention are:

[0046] (1) The flower-shaped LiVPO4F positive electrode material prepared by nano-design control has uniform morphology and high crystallinity.

[0047] (2) The LiVPO4F positive electrode material obtained by the present invention has excellent electrochemical properties, and the specific capacity can reach 132.6 mAh / g, which makes the material have high use value and can meet the needs of power lithium batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 is the XRD pattern of the sample in Example 1 of the present invention;

[0049] Figure 2 This is a SEM image of the sample in Example 1 of the present invention;

[0050] Figure 3 is the physical adsorption curve of the sample in Example 1 of the present invention;

[0051] Figure 4 This is the charge and discharge curve of the sample in Example 1 of the present invention. DETAILED DESCRIPTION

[0052] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0053] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0054] In the examples of the present application, an X-ray powder diffractometer was used to observe the structure of the sample, and a scanning electron microscope was used to observe the morphology of the sample.

[0055] Instruments: scanning electron microscope (Quanta 200F), X-ray powder diffractometer (SmartLab), blue electric tester (LAND CT2001A), physical adsorption instrument (Autosorb iQ).

[0056] The method of flower-shaped LiVPO4F battery positive electrode material specifically comprises the following steps:

[0057] (1) Mix a vanadium source and a phosphorus source in a molar ratio of 1:1, disperse in water, and stir magnetically at room temperature for one hour;

[0058] (2) hydroheating the dispersion obtained in step (1) at 100-180° C. for 10-24 h to obtain an intermediate product 1;

[0059] (3) The intermediate product 1 prepared in step (2) is dispersed in isobutanol, stirred at 30-70°C for 3 hours, and then refluxed at 100-150°C for 5-20 hours. The refluxed product is treated in a H2 / Ar reducing atmosphere at 600-1000°C for 1-10 hours to obtain the intermediate product 2;

[0060] (4) The intermediate product 2 prepared in step (3), the fluorine source and the lithium source are mixed in a molar ratio of 1:1:1 and ball-milled for 1 to 10 hours, and then sintered at 500 to 800° C. in an inert atmosphere for 1 to 10 hours to obtain a flower-shaped LiVPO4F positive electrode material.

[0061] Charge and discharge test system

[0062] The electrochemical test instrument used in this experiment is the LAND CT2001A

[0063] Charge and discharge test method

[0064] This experiment adopts the rate charge and discharge test method, and the test is carried out at a current density of 0.2~20C, where 1C=156mA g -1 .

[0065] Example 1

[0066] Vanadium pentoxide, phosphoric acid and lithium fluoride are used as initial raw materials. First, weigh 2.4g of vanadium pentoxide and disperse it in 57.7mL of distilled water, add 2.98g of phosphoric acid, stir at room temperature for one hour, then transfer to a 100mL hydrothermal kettle and react at 120℃ for 16h. The products obtained after hydrothermal treatment are centrifuged and washed three times with hydrated acetone, the centrifugal speed is 6000rpm, and the centrifugal time is 5 minutes each time, and then dried in a vacuum drying oven at 70℃ for 12h to obtain intermediate product 1. Weigh 2g of intermediate product 1 and add it to 50mL of isobutanol, stir at room temperature for 1h, then stir at 50℃ for 3h, reflux at 110℃ for 10h, wash the refluxed product with ethanol centrifugation three times, then dry it in a vacuum drying oven at 70℃ for 12h, and treat the refluxed product at 800℃ for 2h in a mixed atmosphere of hydrogen and argon (wherein the hydrogen concentration is 10vol%) to obtain intermediate product 2. 1.14 g of intermediate product 2 was weighed and mixed with 0.21 g of LiF and ball-milled for 4 h at a ball-milling speed of 300 rpm. The ball-milled product was sintered at 650° C. for 2 h in an argon atmosphere in a tube furnace and naturally cooled to room temperature to obtain flower-like LiVPO4F. Figure 1 The X-ray diffraction pattern of the obtained product shows that it is LiVPO4F, has no other impurities, and has high crystallinity. Figure 2 Scanning electron microscopy revealed that LiVPO4F is a nanoflower (10μm) assembled from ultrathin nanosheets (20nm). Figure 3 It can be seen that the prepared LiVPO4F exhibits a 20m2 g -1 The specific surface area of ​​the product LiVPO4F was prepared with a pore size distribution of 2-5nm, a conductive agent Ketjen black and a binder PVDF in a mass ratio of 8:1:1 to prepare a 1.5mg / cm 2 The positive electrode sheet is matched with a commercial lithium sheet as the negative electrode, and the electrolyte with LiPF6 as the solute, ethylene carbonate (EC), and diethyl carbonate (DEC) (EC:DEC = 1:1 vol%) as the solvent is assembled into a lithium-ion battery button cell. The lithium battery is assembled in the order of positive electrode shell / electrode sheet / polypropylene diaphragm / lithium sheet / gasket / negative electrode shell. The charge and discharge test was carried out at a current density of 0.2C, and the first discharge specific capacity was 132.6mAh / g.

[0067] Example 2

[0068] Vanadium pentoxide, ammonium dihydrogen phosphate and lithium fluoride are used as initial raw materials. First, weigh 2.4g of vanadium pentoxide and disperse it in 57.7mL of distilled water, add 1.52g of ammonium dihydrogen phosphate, stir at room temperature for one hour, then transfer to a 100mL hydrothermal kettle and react at 120℃ for 16h. The products obtained after hydrothermal treatment are centrifuged and washed three times with hydrated acetone, the centrifugal speed is 6000rpm, and the centrifugal time is 5 minutes each time, and then dried in a vacuum drying oven at 70℃ for 12h to obtain intermediate product 1. Weigh 2g of intermediate product 1 and add it to 50mL of isobutanol, stir at room temperature for 1h, then stir at 50℃ for 3h, and then reflux at 110℃ for 10h, wash the refluxed product with ethanol centrifugally for 3 times, and then dry it in a vacuum drying oven at 70℃ for 12h, and treat the refluxed product at 800℃ for 2h in a reducing atmosphere of a mixed atmosphere of hydrogen and argon (wherein the hydrogen concentration is 10vol%) to obtain intermediate product 2. 1.14 g of intermediate product 2 was weighed and mixed with 0.21 g of LiF and ball-milled for 4 h at a ball-milling speed of 300 rpm. The ball-milled product was sintered at 650 ° C for 2 h in an argon atmosphere in a tube furnace and naturally cooled to room temperature to obtain flower-shaped LiVPO4F. The electrochemical performance of this sample is similar to that of LiVPO4F in Example 1, with a specific capacity of 130 mAh / g.

[0069] Example 3

[0070] Vanadium pentoxide, ammonium dihydrogen phosphate, lithium carbonate and ammonium fluoride are used as initial raw materials. First, weigh 2.4g of vanadium pentoxide and disperse it in 57.7mL of distilled water, add 1.52g of ammonium dihydrogen phosphate, stir at room temperature for one hour, then transfer to a 100mL hydrothermal kettle and react at 120℃ for 16h. The products obtained after hydrothermal treatment are centrifuged and washed three times with hydrated acetone, the centrifugal speed is 6000 rpm, and the centrifugal time is 5 minutes each time, and then dried in a vacuum drying oven at 70℃ for 12h to obtain intermediate product 1. Weigh 2g of intermediate product 1 and add it to 50mL of isobutanol, stir at room temperature for 1h, then stir at 50℃ for 3h, and then reflux at 110℃ for 10h, wash the refluxed product with ethanol centrifugally for 3 times, and then dry it in a vacuum drying oven at 70℃ for 12h, and treat the refluxed product at 800℃ for 2h in a mixed atmosphere of hydrogen and argon (wherein the hydrogen concentration is 10vol%) to obtain intermediate product 2. 1.14 g of intermediate product 2 was weighed and mixed with 0.30 g of Li2CO3 and 0.31 g of NH4F and ball-milled for 4 h at a ball-milling speed of 300 rpm. The ball-milled product was sintered at 650 ° C for 2 h in an argon atmosphere in a tube furnace and naturally cooled to room temperature to obtain flower-shaped LiVPO4F. The electrochemical performance of this sample was similar to that of the LiVPO4F in Example 1, with a specific capacity of 130.2 mAh / g.

[0071] Example 4

[0072] Vanadium pentoxide, phosphoric acid, lithium carbonate and ammonium fluoride are used as initial raw materials. First, weigh 2.4g of vanadium pentoxide and disperse it in 57.7mL of distilled water, add 2.98g of ammonium dihydrogen phosphate, stir at room temperature for one hour, then transfer to a 100mL hydrothermal kettle and react at 120℃ for 16h. The products obtained after hydrothermal treatment are centrifuged and washed three times with hydrated acetone, the centrifugal speed is 6000rpm, and the centrifugal time is 5 minutes each time, and then dried in a vacuum drying oven at 70℃ for 12h to obtain intermediate product 1. Weigh 2g of intermediate product 1 and add it to 50mL of isobutanol, stir at room temperature for 1h, then stir at 50℃ for 3h, reflux at 110℃ for 10h, wash the refluxed product with ethanol centrifugation three times, then dry it in a vacuum drying oven at 70℃ for 12h, and treat the refluxed product at 800℃ for 2h in a mixed atmosphere of hydrogen and argon (wherein the hydrogen concentration is 10vol%) to obtain intermediate product 2. 1.14 g of intermediate product 2 was weighed and mixed with 0.30 g of Li2CO3 and 0.31 g of NH4F and ball milled for 4 h at a ball milling speed of 300 rpm. The ball milled product was sintered at 650 ° C for 2 h in an argon atmosphere in a tube furnace and naturally cooled to room temperature to obtain flower-shaped LiVPO4F. The electrochemical performance of this sample is similar to that of LiVPO4F in Example 1, with a specific capacity of 131.8 mAh / g.

[0073] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A method for preparing a LiVPO4F material, characterized in that: The following steps are involved: 1) Mixing the raw material containing the vanadium source and the phosphorus source with water 1, and performing a hydrothermal reaction to obtain an intermediate product 1; 2) mixing the raw material containing the intermediate product 1 and isobutanol 2, and heating the mixture for reaction to obtain a mixed solution; 3) reflux the mixed solution at 100-150° C. for 5-20 h to obtain a reflux product; 4) treating the reflux product under a reducing atmosphere to obtain an intermediate product 2; 5) mixing and ball-milling the raw materials containing the fluorine source, the lithium source and the intermediate product 2, and sintering them in an inert atmosphere to obtain the LiVPO4F material; The vanadium source is selected from at least one of V2O5, V2O3 or NH4VO3; the phosphorus source is selected from at least one of NH4H2PO4, (NH4)2HPO4 or H3PO4; the lithium source is selected from at least one of Li2CO3, LiOH or LiF; the fluorine source is selected from at least one of LiF or NH4F; The molar ratio of the vanadium source, phosphorus source, fluorine source and lithium source is (0.8-1.2):(0.8-1.2):(0.8-1.2):(0.8-1.2), the molar number of the vanadium source is calculated based on the molar number of the V element in the vanadium source; the molar number of the phosphorus source is calculated based on the molar number of the P element in the phosphorus source; the molar number of the fluorine source is calculated based on the molar number of the F element in the fluorine source; the molar number of the lithium source is calculated based on the molar number of the Li element in the lithium source; In step 1), the temperature of the hydrothermal reaction is 100 to 180°C; the time of the hydrothermal reaction is 10 to 24 hours; In step 2), the heating reaction temperature is 30-70°C and the reaction time is 2-6 hours; In step 4), the reduction treatment is carried out at 600-1000°C for 1-10 h; In step 5), the sintering temperature is 500-800° C. and the sintering time is 1-10 h.

2. The method for preparing the LiVPO4F material according to claim 1, characterized in that: The molar ratio of the vanadium source, the phosphorus source, the fluorine source and the lithium source is 1:1:1:

1.

3. The method for preparing the LiVPO4F material according to claim 1, characterized in that: In step 1), the temperature of the hydrothermal reaction is 120-140°C; the time of the hydrothermal reaction is 15-20 h; the mixing 1 is stirred at 20-30°C for 30-100 min; In step 2), the mixture 2 is stirred at 20-30° C. for 20-60 min; In step 3), the reflux temperature is 100-120°C; the reflux time is 10-15 h; In step 4), the reduction treatment is carried out at 700-850°C for 2-5 hours; The reducing atmosphere contains hydrogen, and the concentration of the hydrogen is 5-10%.

4. The method for preparing the LiVPO4F material according to claim 1, characterized in that: The reducing atmosphere contains hydrogen and an inert gas, and the inert gas is argon.

5. The method for preparing the LiVPO4F material according to claim 1, characterized in that: In step 5), the inert atmosphere is selected from at least one of nitrogen or argon; the ball milling speed is 100-500 rpm; the ball milling time is 1-10 h; the sintering temperature is 650-700 °C; and the sintering time is 2-5 h.

6. The method for preparing the LiVPO4F material according to claim 1, characterized in that: The ball milling speed is 300-400 rpm; the ball milling time is 4-6 h.

7. LiVPO4F material prepared by any method of claims 1-6.

8. Use of the LiVPO4F material according to claim 7 as a positive electrode material for a lithium battery.

9. A positive electrode material for a lithium battery, characterized in that: The positive electrode material contains the LiVPO4F material according to claim 7, and the content of LiVPO4F in the positive electrode material is 50-90 wt%. 10 . The positive electrode material for lithium battery according to claim 9 , wherein the electrode material further comprises a conductive agent and a binder; the conductive agent is Ketjen black; and the binder is polyvinylidene fluoride.