Cross-linked polysulfone anion exchange membrane with high quaternary ammonium content and preparation method thereof
Through the cross-linked polysulfone anion exchange membrane with high quaternary ammonium content, a three-dimensional network structure is constructed using chloromethylation and quaternization reactions, which solves the problem of difficulty in balancing the conductivity and alkali resistance of the anion exchange membrane and achieves high efficiency. Excellent hydroxide ion conductivity and dimensional stability, suitable for high-performance fuel cells.
Patent Information
- Application Number
- CN202310108082.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-14
AI Technical Summary
While existing high-performance anion exchange membranes improve hydroxide ion conductivity, it is difficult to maintain dimensional stability and alkali resistance, which affects the service life of fuel cells.
A cross-linked polysulfone anion exchange membrane with high quaternary ammonium content is used. Through chloromethylation, quaternization and chemical cross-linking reactions, a polysulfone membrane with a three-dimensional network structure is constructed to improve ion conductivity and dimensional stability. And enhance alkali resistance through impregnation treatment.
Significantly improves the ion exchange capacity and conductivity of the anion exchange membrane, reduces the water swelling rate, enhances dimensional stability and alkali resistance, balances the relationship between conductivity, stability and alkali resistance, and is suitable for high performance fuel cells.
Smart Images

Figure CN115975197B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alkaline fuel cell anion exchange membrane preparation, and in particular relates to a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content, and also relates to a preparation method of the cross-linked polysulfone anion exchange membrane. Background Art
[0002] Fuel cells are a new type of clean and efficient energy source that can efficiently convert chemical energy into electrical energy and only produce water and a small amount of carbon dioxide during operation. They have a bright future. As the first practical fuel cell, alkaline fuel cells use non-platinum metals as catalysts and have the advantages of low cost, fast electrode reaction speed and strong tolerance to carbon monoxide. As one of its core components, the anion exchange membrane is OH - It provides a channel for conduction while effectively isolating fuel gas and oxygen.
[0003] High-performance fuel cells depend to a large extent on the development of high-performance anion exchange membranes. Currently, the development of high-performance anion exchange membranes faces the prominent problem of balancing hydroxide ion conductivity, dimensional stability and alkali resistance. In order to obtain high conductivity, dimensional stability and alkali resistance must be sacrificed, which will seriously affect the service life of the fuel cell. Polysulfone (PS) is a high-performance polymer with a sulfone group in the main chain. It has excellent antioxidant stability, heat resistance, acid and alkali corrosion resistance, etc. PS is used as the basic material, and a chain segment is introduced from the side chain to bond the quaternary ammonium group to prepare a quaternized polysulfone with a high quaternary ammonium group. At the same time, a polysulfone anion exchange membrane with a high quaternary ammonium content and a three-dimensional network structure is formed through a chemical cross-linking reaction. It has high ion conductivity and dimensional stability. Summary of the invention
[0004] The purpose of the present invention is to provide a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content, which solves the problems of poor dimensional stability and alkali resistance of traditional anion exchange membranes at high proton conductivity.
[0005] Another object of the present invention is to provide a method for preparing the cross-linked polysulfone anion exchange membrane.
[0006] The technical solution adopted by the present invention is a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content, and its structural formula is:
[0007]
[0008] Another technical solution adopted by the present invention is a method for preparing a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content, which is specifically implemented according to the following steps:
[0009] Step 1, preparing chloromethylated polysulfone;
[0010] Step 2, preparing a quaternized polysulfone containing an amino group at the end;
[0011] Step 3, preparing a linear polysulfone membrane material with a high quaternary ammonium content in the side chain;
[0012] Step 4, preparing a cross-linked polysulfone membrane material with a high quaternary ammonium content;
[0013] Step 5: immerse the cross-linked polysulfone membrane material in a 1 mol / L NaOH solution for 24 hours to obtain a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content.
[0014] The present invention is also characterized in that:
[0015] In step 1, specifically:
[0016] PS is dissolved in dichloromethane, and after it is dissolved, a catalyst SnCl4 is added, and 1,4-dichloromethoxybutane is dropped with a dropping funnel. The reaction is carried out at 40-60°C for 24-36 hours, and then 2-4 mol / L of dilute hydrochloric acid is added to the reaction mixture, and then a precipitant is added to precipitate the product, and the product is allowed to stand, separated, washed, and dried to obtain chloromethylated polysulfone.
[0017] In step 2, specifically: dissolving the chloromethylated polysulfone in DMF, then adding 3-N,N-dimethylaminopropylamine, reacting at room temperature for 24 hours, adding isopropanol precipitant for precipitation after the reaction, centrifuging, washing and drying to obtain quaternized polysulfone;
[0018] The mass ratio of chloromethylated polysulfone, DMF and 3-N,N-dimethylaminopropylamine is 1:50:1.6.
[0019] In step 3, specifically: dissolving the quaternized polysulfone with DMSO, adding 2,3-epoxypropyltrimethylammonium chloride after the polysulfone is dissolved and fully reacting for 24 hours, and then precipitating with anhydrous ethanol, centrifuging, washing and drying to obtain a linear polysulfone membrane material with a high quaternary ammonium content in the side chain;
[0020] The mass ratio of quaternized polysulfone, DMSO and 2,3-epoxypropyltrimethylammonium chloride is 1:55:2.08.
[0021] In step 4, specifically, the linear polysulfone membrane material is dissolved in dimethyl sulfoxide, the temperature is lowered to room temperature after it is fully dissolved, glutaraldehyde is added as a cross-linking agent, and then concentrated sulfuric acid is added as a catalyst, stirred evenly, poured into a watch glass by a solution casting method to react for 12 hours, and then the mixed solution is dried at 50-60° C., and after the solvent is removed, distilled water is added for demolding treatment, and finally the film is washed with distilled water 3 times to obtain a cross-linked polysulfone membrane material with a high quaternary ammonium content;
[0022] Among them, the mass ratio of linear polysulfone membrane material, dimethyl sulfoxide, glutaraldehyde and concentrated sulfuric acid is 1:44:1.38:0.075.
[0023] The beneficial effects of the present invention are as follows: the cross-linked polysulfone anion exchange membrane prepared by the method of the present invention greatly improves the ion exchange capacity and ion conductivity of the anion exchange membrane. Since the quaternary ammonium group is far away from the polysulfone main chain, the water absorption swelling rate of the polysulfone main chain is reduced, and the dimensional stability is improved. At the same time, the spatial network structure is formed by chemical cross-linking, the compactness of the anion exchange membrane is enhanced, the resistance of free radicals entering the interior of the membrane is increased, the dimensional stability and alkali resistance are improved, and the relationship between ion conductivity, dimensional stability and alkali resistance is balanced. Among them, the ion exchange capacity of the CPS-QN membrane with the highest quaternary ammonium group content reaches 1.72mmol / g, the water absorption rate at 25℃ and 85℃ reaches 38.7% and 63.2%, but the corresponding water absorption swelling is only 14.4% and 28.4%, the hydroxide ion conductivity reaches 41mS / cm and 116mS / cm, and the conductivity retention after immersion in strong alkali for 600h reaches 83.8%. It maintains good dimensional stability and alkali resistance at high conductivity and is expected to be used in fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is an infrared spectrum of the CPS-QN film prepared by the method of the present invention;
[0025] Figure 2 is a curve diagram showing the water absorption rate of the CPS-QN film prepared by the method of the present invention as a function of temperature;
[0026] Figure 3 is a curve diagram showing the change of swelling rate of the CPS-QN film prepared by the method of the present invention as a function of temperature;
[0027] Figure 4 is the OH of the CPS-QN film prepared by the method of the present invention - Conductivity versus temperature graph;
[0028] Figure 5 It is a graph showing the ion conductivity retention rate of the CPS-QN membrane prepared by the method of the present invention. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0030] The method for preparing a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content of the present invention is specifically implemented according to the following steps:
[0031] Step 1, preparing chloromethylated polysulfone (CMPS); specifically as follows:
[0032] PS is dissolved in dichloromethane, and after it is dissolved, a catalyst SnCl4 is added, and 1,4-dichloromethoxybutane is dropped through a dropping funnel, and the reaction is carried out at 40-60°C for 24-36 hours, and then 2-4 mol / L of dilute hydrochloric acid is added to the reaction mixture, and then a precipitant is added to precipitate the product, and the product is allowed to stand, separated, washed, and dried to obtain chloromethylated polysulfone (CMPS);
[0033] The mass ratio of polysulfone, dichloromethane, 1,4-dichloromethoxybutane and tin tetrachloride is 1:47:1.9:0.58;
[0034] The precipitant is any one or more of anhydrous ethanol, methanol, and isopropanol.
[0035] The preparation method of 1,4-dichloromethoxybutane is specifically as follows: 1,4-butanediol and formaldehyde are uniformly mixed, phosphorus trichloride solution is added dropwise at 0°C, after the addition is completed, the mixture is reacted at 10°C for 12 hours, then the mixed solution is transferred to a separatory funnel for stratification, and the supernatant is dried over anhydrous magnesium sulfate to obtain 1,4-dichloromethoxybutane;
[0036] The chemical reaction equation for preparing CMPS is shown in formula (1):
[0037]
[0038] Step 2, preparing a quaternized polysulfone (PS-QN) containing an amino group at the end;
[0039] The chemical reaction equation for preparing quaternized polysulfone (PS-QN) is shown in formula (2):
[0040]
[0041] Specifically, chloromethylated polysulfone (CMPS) was dissolved in DMF, and then 3-N,N-dimethylaminopropylamine was added to react at room temperature for 24 hours. After the reaction, isopropanol precipitant was added to precipitate, centrifuged, washed and dried to obtain quaternary ammonium polysulfone (PS-QN);
[0042] The mass ratio of chloromethylated polysulfone, DMF and 3-N,N-dimethylaminopropylamine is 1:50:1.6;
[0043] Step 3, preparing a linear polysulfone membrane material (HPS-QN) with a high quaternary ammonium content in the side chain;
[0044] Specifically, the quaternized polysulfone obtained in step 2 is dissolved in DMSO, and after the quaternary ammonium polysulfone is dissolved, 2,3-epoxypropyltrimethylammonium chloride (M is 152) is added to fully react for 24 hours, and then precipitated with anhydrous ethanol, centrifuged, washed and dried to obtain a linear polysulfone membrane material with a high quaternary ammonium content in the side chain;
[0045] The mass ratio of quaternized polysulfone, DMSO and 2,3-epoxypropyltrimethylammonium chloride is 1:55:2.08;
[0046] The chemical reaction equation for preparing the linear polysulfone membrane material (HPS-QN) with high quaternary ammonium content in the side chain is shown in formula (3):
[0047]
[0048] Step 4, preparing a cross-linked polysulfone membrane material (CPS-QN) with a high quaternary ammonium content;
[0049] Specifically, the linear polysulfone membrane prepared in step 3 is dissolved in dimethyl sulfoxide, and the temperature is lowered to room temperature after it is fully dissolved, glutaraldehyde is added as a cross-linking agent, and then concentrated sulfuric acid is added as a catalyst, and stirred evenly, and poured into a watch glass by a solution casting method to react for 12 hours, and then the mixed solution is dried at 50-60°C, and after the solvent is removed, distilled water is added for film removal, and finally the film is washed with distilled water for 3 times to obtain a cross-linked polysulfone membrane with a high quaternary ammonium content (CPS-QN), which is placed in water for standby use;
[0050] Among them, the mass ratio of linear polysulfone membrane material, dimethyl sulfoxide, glutaraldehyde and concentrated sulfuric acid is 1:44:1.38:0.075.
[0051] The chemical reaction equation for preparing cross-linked polysulfone membrane (CPS-QN) is shown in formula (4):
[0052]
[0053] Step 5: immerse the cross-linked polysulfone membrane material in a 1 mol / L NaOH solution for 24 hours to construct a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content (CHPS-HN).
[0054] The chemical reaction equation for preparing the cross-linked polysulfone anion exchange membrane (CHPS-HN) is shown in formula (5):
[0055]
[0056] The method of the invention uses polysulfone as a basis, introduces quaternary ammonium groups through a quaternization reaction, and increases the content of quaternary ammonium groups through secondary introduction of quaternary ammonium groups. At the same time, a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content is constructed through chemical cross-linking. The prepared anion exchange membrane can still maintain good alkali resistance and dimensional stability under high ion conductivity, thereby solving the problem of difficulty in balancing the ion conductivity, dimensional stability and alkali resistance of the anion exchange membrane.
[0057] Example 1
[0058] The method for preparing a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content of the present invention is specifically implemented according to the following steps:
[0059] Step 1, dissolving PS in dichloromethane, adding catalyst SnCl4 after dissolution, and dropping 1,4-dichloromethoxybutane with a dropping funnel, reacting at 40°C for 24h, then adding 2mol / L dilute hydrochloric acid to the reaction mixture, and then adding a precipitant to precipitate the product, standing, separating, washing, and drying to obtain chloromethylated polysulfone (CMPS);
[0060] The mass ratio of polysulfone, dichloromethane, 1,4-dichloromethoxybutane and tin tetrachloride is 1:47:1.9:0.58; and the precipitant is anhydrous ethanol.
[0061] Step 2, dissolving the chloromethylated polysulfone in DMF, then adding 3-N,N-dimethylaminopropylamine, reacting at room temperature for 24 hours, adding isopropanol precipitant for precipitation after the reaction, centrifuging, washing and drying to obtain quaternized polysulfone (PS-QN);
[0062] The mass ratio of chloromethylated polysulfone, DMF and 3-N,N-dimethylaminopropylamine is 1:50:1.6;
[0063] Step 3, dissolving the quaternized polysulfone obtained in step 2 with DMSO, adding 2,3-epoxypropyltrimethylammonium chloride after dissolution to fully react for 24 hours, and then precipitating with anhydrous ethanol, centrifuging, washing and drying to obtain a linear polysulfone membrane material with a high quaternary ammonium content in the side chain;
[0064] The mass ratio of quaternized polysulfone, DMSO and 2,3-epoxypropyltrimethylammonium chloride is 1:55:2.08;
[0065] Step 4, dissolving the linear polysulfone membrane material prepared in step 3 in dimethyl sulfoxide, lowering the temperature to room temperature after fully dissolved, adding glutaraldehyde as a cross-linking agent, and then adding concentrated sulfuric acid as a catalyst, stirring evenly, pouring into a watch glass by solution casting method to react for 12 hours, and then drying the mixed solution at 50° C. After the solvent is removed, adding distilled water for film removal, and finally washing the film with distilled water for 3 times to obtain a cross-linked polysulfone membrane material (CPS-QN) with a high quaternary ammonium content, which is placed in water for standby use;
[0066] Among them, the mass ratio of linear polysulfone membrane material, dimethyl sulfoxide, glutaraldehyde and concentrated sulfuric acid is 1:44:1.38:0.075.
[0067] Step 5: immerse the cross-linked polysulfone membrane material in a 1 mol / L NaOH solution for 24 hours to construct a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content (CHPS-HN).
[0068] Example 2
[0069] The method for preparing a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content of the present invention is specifically implemented according to the following steps:
[0070] Step 1, dissolving PS in dichloromethane, adding catalyst SnCl4 after dissolution, and dropping 1,4-dichloromethoxybutane with a dropping funnel, reacting at 50° C. for 30 hours, then adding 4 mol / L dilute hydrochloric acid to the reaction mixture, and then adding a precipitant to precipitate the product, standing, separating, washing, and drying to obtain chloromethylated polysulfone (CMPS);
[0071] The mass ratio of polysulfone, dichloromethane, 1,4-dichloromethoxybutane and tin tetrachloride is 1:47:1.9:0.58; and the precipitant is a mixture of methanol and isopropanol.
[0072] Step 2, dissolving chloromethylated polysulfone (CMPS) in DMF, then adding 3-N,N-dimethylaminopropylamine, reacting at room temperature for 24 hours, adding isopropanol precipitant for precipitation after the reaction, centrifuging, washing and drying to obtain quaternized polysulfone (PS-QN);
[0073] The mass ratio of chloromethylated polysulfone, DMF and 3-N,N-dimethylaminopropylamine is 1:50:1.6;
[0074] Step 3, dissolving the quaternized polysulfone obtained in step 2 with DMSO, adding 2,3-epoxypropyltrimethylammonium chloride after dissolution to fully react for 24 hours, and then precipitating with anhydrous ethanol, centrifuging, washing and drying to obtain a linear polysulfone membrane material with a high quaternary ammonium content in the side chain;
[0075] The mass ratio of quaternized polysulfone, DMSO and 2,3-epoxypropyltrimethylammonium chloride is 1:55:2.08;
[0076] Step 4, dissolving the linear polysulfone membrane material prepared in step 3 in dimethyl sulfoxide, lowering the temperature to room temperature after fully dissolved, adding glutaraldehyde as a cross-linking agent, and then adding concentrated sulfuric acid as a catalyst, stirring evenly, pouring into a watch glass by solution casting method to react for 12 hours, and then drying the mixed solution at 55° C. After the solvent is removed, adding distilled water for film removal, and finally washing the film with distilled water for 3 times to obtain a cross-linked polysulfone membrane material (CPS-QN) with a high quaternary ammonium content, which is placed in water for standby use;
[0077] Among them, the mass ratio of linear polysulfone membrane material, dimethyl sulfoxide, glutaraldehyde and concentrated sulfuric acid is 1:44:1.38:0.075.
[0078] Step 5: immerse the cross-linked polysulfone membrane material in a 1 mol / L NaOH solution for 24 hours to construct a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content (CHPS-HN).
[0079] Example 3
[0080] The method for preparing a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content of the present invention is specifically implemented according to the following steps:
[0081] Step 1, dissolving PS in dichloromethane, adding catalyst SnCl4 after dissolution, and dropping 1,4-dichloromethoxybutane with a dropping funnel, reacting at 60° C. for 36 hours, then adding 3 mol / L dilute hydrochloric acid to the reaction mixture, and then adding a precipitant to precipitate the product, standing, separating, washing, and drying to obtain chloromethylated polysulfone (CMPS);
[0082] The mass ratio of polysulfone, dichloromethane, 1,4-dichloromethoxybutane and tin tetrachloride is 1:47:1.9:0.58; and the precipitant is isopropanol.
[0083] The preparation method of 1,4-dichloromethoxybutane is specifically as follows: 1,4-butanediol and formaldehyde are uniformly mixed, phosphorus trichloride solution is added dropwise at 0°C, after the addition is completed, the mixture is reacted at 10°C for 12 hours, then the mixed solution is transferred to a separatory funnel for stratification, and the supernatant is dried over anhydrous magnesium sulfate to obtain 1,4-dichloromethoxybutane;
[0084] Step 2, dissolving chloromethylated polysulfone (CMPS) in DMF, then adding 3-N,N-dimethylaminopropylamine, reacting at room temperature for 24 hours, adding isopropanol precipitant for precipitation after the reaction, centrifuging, washing and drying to obtain quaternized polysulfone (PS-QN);
[0085] The mass ratio of chloromethylated polysulfone, DMF and 3-N,N-dimethylaminopropylamine is 1:50:1.6;
[0086] Step 3, dissolving the quaternized polysulfone obtained in step 2 with DMSO, adding 2,3-epoxypropyltrimethylammonium chloride after dissolution to fully react for 24 hours, and then precipitating with anhydrous ethanol, centrifuging, washing and drying to obtain a linear polysulfone membrane material with a high quaternary ammonium content in the side chain;
[0087] The mass ratio of quaternized polysulfone, DMSO and 2,3-epoxypropyltrimethylammonium chloride is 1:55:2.08;
[0088] Step 4, dissolving the linear polysulfone membrane material prepared in step 3 in dimethyl sulfoxide, lowering the temperature to room temperature after fully dissolved, adding glutaraldehyde as a cross-linking agent, and then adding concentrated sulfuric acid as a catalyst, stirring evenly, pouring into a watch glass by solution casting method to react for 12 hours, and then drying the mixed solution at 60° C. After the solvent is removed, adding distilled water for film removal, and finally washing the film with distilled water for 3 times to obtain a cross-linked polysulfone membrane material (CPS-QN) with a high quaternary ammonium content, which is placed in water for standby use;
[0089] Among them, the mass ratio of linear polysulfone membrane material, dimethyl sulfoxide, glutaraldehyde and concentrated sulfuric acid is 1:44:1.38:0.075.
[0090] Step 5: immerse the cross-linked polysulfone membrane material in a 1 mol / L NaOH solution for 24 hours to construct a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content (CHPS-HN).
[0091] The infrared spectra of CMPS, HPS-QN and CPS-QN prepared by the method of the present invention are as follows: Figure 1 As shown in the infrared spectrum of chloromethylated polysulfone, 1080cm -1 , 1325cm -1 With 1295cm -1 It is the characteristic absorption peak of -SO2- group, 1245cm -1 With 1015cm -1 It is the antisymmetric and symmetric stretching vibration absorption peak of aromatic ether, 1585cm -1 With 1490cm -1 The peak at 670 cm is the characteristic absorption peak of the benzene ring. -1 The characteristic absorption peak of chloromethyl is at 3441cm; in the infrared spectrum of HPS-QN, in addition to the characteristic absorption peak of polysulfone, the characteristic absorption peak of hydroxyl group appears at 1636cm -1 The characteristic absorption peak of the quaternary ammonium group appears at 1636 cm-1. -1 and 3441cm -1 There are also characteristic absorption peaks of ether bonds at 1263 cm -1 ,1096cm -1 and 1033cm -1 Place.
[0092] The CPS-QN membrane was soaked in 0.01mol / L dilute hydrochloric acid (V1) for 36h. After that, the mixture was titrated with 0.01mol / L NaOH solution using phenolphthalein as an indicator. The consumed volume was V2. The IEC of the anion exchange membrane was calculated by (C1V1-C2V2) / m. CMPS with different chlorine contents were prepared by controlling the chloromethylation time. Then, a series of anion exchange membranes with different IEC were prepared. According to the different IEC, the membranes were recorded as CPS-QN-1 (IEC was 1.11mmol / g), CPS-QN-2 (IEC was 1.39mmol / g) and CPS-QN-3 (IEC was 1.71mmol / g) to study the performance changes.
[0093] The water absorption rate of CPS-QN film varies with temperature, as shown in the figure. Figure 2 As shown in the figure, the working environment of the anion exchange membrane is in the electrolyte solution. The anion exchange membrane absorbs water to form quaternary ammonium hydrated ion clusters, which are connected to each other to form channels, thereby conducting hydroxide ions. It can be seen from the figure that the CPS-QN membrane exhibits a good water absorption rate, which is related to its molecular structure. The CPS-QN membrane not only has hydrophilic quaternary ammonium groups, but also has hydrophilic ether bonds, which are conducive to the absorption of water. With the increase of quaternary ammonium content, the water absorption rate increases. The water absorption rate of the CPS-QN-3 membrane at room temperature and 85°C is as high as 38.7% and 63.2%, showing excellent water absorption capacity, which is much higher than the water absorption rate of the commercial Nafion115 membrane (28.6% and 42.7%, respectively).
[0094] The water absorption rate of CPS-QN film varies with temperature, as shown in the figure. Figure 3 As shown in the figure, the water absorption swelling rate of CPS-QN membrane increases with the increase of temperature, which is consistent with the change of water absorption rate of CPS-QN membrane. As the temperature increases, the mobility of quaternary ammonium groups and water molecules increases, and it is easier to combine water to form hydrated ion clusters, the water absorption capacity increases, and thus the swelling rate is bound to increase. At the same temperature, with the increase of IEC, the water absorption rate increases. Although the water absorption rate of CPS-QN-3 is the largest, the water absorption swelling rate of CPS-QN-3 membrane at room temperature and 85°C is only 14.4% and 28.4%, which is much lower than the performance of Nafion115 under the same conditions (24.9% and 55%). This is related to their cross-linked structure. CPS-QN membrane can form a spatial network structure through chemical cross-linking, which improves the mechanical properties of anion exchange membrane, increases the density of the membrane, and increases the resistance of water molecules entering the membrane, thereby enhancing the dimensional stability of the anion exchange membrane.
[0095] OH of CPS-QN film - The conductivity curve is as follows: Figure 4As shown, the hydroxide ion conductivity, as one of the most core properties of anion exchange membranes, directly determines the performance of anion exchange membrane fuel cells. As can be seen from the figure, the hydroxide ion conductivity of the three anion exchange membranes increases with the increase in temperature, which is related to the increase in the mobility of hydrated ion clusters. With the increase in the content of quaternary ammonium groups, the ion conductivity of the corresponding anion exchange membrane is enhanced. Among them, the hydroxide ion conductivity of CPS-PA-3 at room temperature and 85°C is 41mS / cm and 116mS / cm, respectively, which can meet the minimum requirement of fuel cells for ion conductivity (0.01S / cm) and has good ion conductivity.
[0096] The working environment of anion exchange membrane is in alkaline solution. Long-term alkaline working environment causes the anion exchange membrane to rupture, reduces the conductivity of hydroxide ions, and seriously affects the use of anion exchange membrane fuel cells. Therefore, high-performance anion exchange membranes must have excellent alkali resistance. The CPSF-HN membrane is immersed in 80°C KOH solution, and the immersion time is controlled. The alkali resistance of the anion exchange membrane is measured by measuring the retention rate of the ion conductivity of the membrane material. The alkali resistance stability curve of the CPSF-HN membrane is shown in the figure below. Figure 5 As shown in the figure, the CPS-PA membrane can form a spatial network structure, which improves the mechanical properties of the anion exchange membrane, allowing the anion exchange membrane to maintain good dimensional stability in a long-term strong alkaline solution and have good alkali resistance. After soaking in strong alkali for 600 hours, the hydroxide ion retention rates of the three anion exchange membranes are all greater than 81%, among which the ion conductivity retention rate of the CPSF-PA-3 membrane is 83.8%, which has good alkali resistance.
Claims
1. A method for preparing a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content, characterized in that: Follow the steps below to implement it: Step 1, preparing chloromethylated polysulfone; specifically: Dissolve PS in dichloromethane, add catalyst SnCl4 after it is dissolved, and drop 1,4-dichloromethoxybutane with a dropping funnel, react at 40-60°C for 24-36h, then add 2-4mol / L dilute hydrochloric acid to the reaction mixture, and then add a precipitant to precipitate the product, let it stand, separate, wash, and dry to obtain chloromethylated polysulfone; the precipitant is any one or more of anhydrous ethanol, methanol, and isopropanol; Step 2, preparing a quaternary ammonium polysulfone containing an amino group at the end; specifically, dissolving the chloromethylated polysulfone in DMF, then adding 3-dimethylaminopropylamine, reacting at room temperature for 24 hours, adding isopropanol precipitant for precipitation after the reaction, centrifuging, washing and drying to obtain the quaternary ammonium polysulfone; The mass ratio of chloromethylated polysulfone, DMF and 3-dimethylaminopropylamine is 1:50:1.6; Step 3, preparing a linear polysulfone membrane material with a high quaternary ammonium content in the side chain; specifically, dissolving the quaternized polysulfone with DMSO, adding 2,3-epoxypropyltrimethylammonium chloride after the polysulfone is dissolved and reacting for 24 hours, precipitating with anhydrous ethanol, centrifuging, washing and drying to obtain a linear polysulfone membrane material with a high quaternary ammonium content in the side chain; The mass ratio of quaternized polysulfone, DMSO and 2,3-epoxypropyltrimethylammonium chloride is 1:55:2.08; Step 4, preparing a cross-linked polysulfone membrane material with a high quaternary ammonium content; specifically, dissolving the linear polysulfone membrane material in dimethyl sulfoxide, lowering the temperature to room temperature after it is fully dissolved, adding glutaraldehyde as a cross-linking agent, and then adding concentrated sulfuric acid as a catalyst, stirring evenly, pouring it into a watch glass by a solution casting method to react for 12 hours, and then drying the mixed solution at 50-60° C., adding distilled water for film removal after the solvent is removed, and finally washing the film with distilled water 3 times to obtain a cross-linked polysulfone membrane material with a high quaternary ammonium content; Among them, the mass ratio of linear polysulfone membrane material, dimethyl sulfoxide, glutaraldehyde and concentrated sulfuric acid is 1:44:1.38:0.075; Step 5: immerse the cross-linked polysulfone membrane material in a 1 mol / L NaOH solution for 24 hours to obtain a cross-linked polysulfone anion exchange membrane with a high quaternary ammonium content.