A low-noise friction material, its preparation method and application
By modifying low-noise friction materials of components such as phenolic resin and modified gel vermiculite, combined with the multi-branched and multi-tening structure of aramid fiber, the stability of brake noise and high-temperature friction coefficient in the prior art is solved, and the stability of brake noise and high-temperature friction coefficient in the existing technology is achieved. Low noise, wear-resistant brake pad performance.
Patent Information
- Application Number
- CN202211581105.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-09
AI Technical Summary
While reducing brake noise, existing friction materials are difficult to maintain stable friction coefficient and wear resistance at high temperatures. The reduction of heavy metals leads to accelerated wear, which cannot meet the performance requirements of new energy vehicles for low-noise brake pads.
Low noise friction materials using modified phenolic resin, aramid fiber, potassium titanate whiskers, glass fiber, modified gel vermiculite, rubber powder, graphite, alumina and barium sulfate, and modified gel The preparation method and hot pressing process of vermiculite combine the multi-branched multi-tenedge structure of aramid fiber to fill and link the pores of the friction material matrix to improve wear resistance and stability of friction coefficient.
It significantly reduces braking noise, improves braking comfort, maintains the stability of the friction coefficient of the brake pads at room temperature and high temperature, reduces the wear of friction materials, improves wear resistance, and meets the low noise and low noise of new energy vehicles. High performance requirements.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of friction material preparation, and in particular to a low-noise friction material and a preparation method and application thereof. Background Art
[0002] Any mechanical equipment and various moving vehicles must have a brake or transmission device. Friction materials are key materials in such brake or transmission devices. Their function is to absorb or transmit power through friction, such as clutch plates transmitting power and brake pads absorbing kinetic energy. The performance of friction materials is directly related to the reliability and stability of vehicle operation. At present, friction materials are often composed of multi-component composite materials such as polymer binders (resins or rubbers), reinforcing fibers, friction performance regulators and other compounding agents. They are required to have sufficient and stable friction coefficients, small differences between dynamic and static friction coefficients, good thermal conductivity and certain high-temperature mechanical strength, good wear resistance and anti-adhesion, and can meet the performance requirements of vehicle or mechanical transmission and braking. In recent years, with the rapid development and popularization of new energy vehicles, since new energy vehicles have no engines and use motors instead, they almost do not generate noise during driving, which puts forward new requirements for friction materials, namely, improving braking or braking noise. Low-noise brake pads have become an important performance indicator of friction materials for new energy vehicle brake pads.
[0003] At present, a series of studies have been conducted to improve the noise problem of brake pad friction materials, mainly by reducing metal components and adding noise reduction components, and some progress has been made. However, with the continuous advancement of technology, higher requirements are placed on the performance of friction materials, and these methods have gradually exposed some shortcomings. Among them, the reduction of metal components will directly lead to an increase in noise reduction components related to the porosity of the friction matrix, causing the wear of the brake pad to accelerate at room temperature and high temperature, and the friction coefficient to decay rapidly. It is impossible to achieve a stable friction coefficient and stable small wear at high temperature. Therefore, it is necessary to find safer and more effective friction materials to replace heavy metals while ensuring the performance of the brake pads, so as to meet the requirements of noise reduction, wear resistance and stable friction coefficient. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a low-noise friction material and a preparation method thereof, and provides the application of the low-noise friction material in the preparation of brake pads or brake pads, aiming to solve some of the problems in the prior art or at least alleviate some of the problems in the prior art.
[0005] To achieve the above object, the present invention is specifically implemented through the following technical solutions:
[0006] The first aspect of the present invention provides a low-noise friction material, which comprises the following components, measured by mass: 5-20 parts of modified phenolic resin, 2-10 parts of aramid fiber, 1-4 parts of potassium titanate whisker, 5-15 parts of glass fiber, 3-15 parts of modified gel vermiculite, 3-7 parts of rubber powder, 15-30 parts of graphite, 2-10 parts of aluminum oxide and 20-40 parts of barium sulfate; wherein the modified gel vermiculite is prepared by mixing gel vermiculite with petroleum coke particles.
[0007] Furthermore, the following components are included, by mass: 14 parts of modified phenolic resin, 5 parts of aramid fiber, 2 parts of potassium titanate whisker, 5 parts of glass fiber, 6 parts of modified gel vermiculite, 3 parts of rubber powder, 25 parts of graphite, 10 parts of aluminum oxide and 30 parts of barium sulfate.
[0008] Furthermore, the modified phenolic resin is cashew nut shell oil modified phenolic resin.
[0009] Furthermore, the preparation method of the modified gel vermiculite comprises:
[0010] S11, mixing water glass and flaky vermiculite in a mass ratio of 7:4;
[0011] S12, adding 1-2% of the mass of the alkali to the mixture of step S11 until gel is generated, placing the gel for aging, and then drying to obtain gel vermiculite;
[0012] S13, uniformly mixing the gel vermiculite and petroleum coke particles in a mass ratio of 7:3 to obtain the modified gel vermiculite.
[0013] Furthermore, the density of the modified gel vermiculite is 0.08-0.2 g / cm 3 , melting point is 1379-1400℃, thermal conductivity is 0.04-0.06kcal / m 2 h℃.
[0014] Furthermore, the particle diameter of the modified gel vermiculite is 0.5-1.5 mm, and further, the particle diameter of the modified gel vermiculite is 0.8 mm.
[0015] The second aspect of the present invention provides S21 as described above, ingredients: weigh each component in proportion, premix the modified gel vermiculite and aramid fiber, then add other components and mix them evenly;
[0016] S22, hot pressing: hot pressing the mixed material in step S21 to obtain a preform;
[0017] S23, post-curing treatment: after drying the preform, post-curing treatment is performed to obtain a low-noise friction material.
[0018] Further, in step S22, the hot pressing molding operation includes: a molding temperature of 160°C, a pre-pressing time of 10s, a pressure relief and exhaust time of 5s, a pressure relief and exhaust number of 5 times, a hot pressing pressure of 10MPa, and a pressing time of 10min.
[0019] Furthermore, in step S23, the post-curing treatment operation includes: keeping the temperature at 160° C. for 10 hours.
[0020] A third aspect of the present invention provides the use of the low-noise friction material as described above in the preparation of brake pads or brake shoes.
[0021] The advantages and positive effects of the present invention are:
[0022] 1. The present invention adopts modified gel vermiculite prepared by mixing gel vermiculite and petroleum coke particles as a functional reinforcing filler. The petroleum coke particles with high porosity adhere to the inside and surface of the gel vermiculite, which increases the porosity of the modified gel vermiculite and is beneficial to improving its sound absorption effect. In combination with other components, it can significantly improve the generation of friction noise of the friction material, so that the brake pad prepared greatly reduces the braking noise and improves the braking comfort.
[0023] 2. The present invention mixes modified gel vermiculite with aramid fiber and other components. On the one hand, petroleum coke particles adhere to the inside and surface of the gel vermiculite to form friction particles of the gel vermiculite, which improves its wear resistance and reduces the wear of the friction material. On the other hand, the aramid fiber is soft in texture, and its multi-branched and multi-tentacle structure can also well fill and link the modified gel vermiculite and the porous gaps on the microstructure of the friction material matrix, which increases the strength and further reduces the wear, maintains the stability of the friction coefficient of the brake pad at room temperature and high temperature, and reduces the wear of the friction material. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the examples. The equipment and reagents used in each embodiment and test example can be obtained from commercial sources unless otherwise specified. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0025] Based on the information contained in this application, it is easy for those skilled in the art to make various changes to the precise description of the present invention without departing from the spirit and scope of the appended claims. It should be understood that the scope of the present invention is not limited to the defined process, properties or components, because these embodiments and other descriptions are only for illustrating specific aspects of the present invention. In fact, various changes that the technicians in this field or related fields can obviously make to the embodiments of the present invention are all covered within the scope of the appended claims.
[0026] In order to better understand the present invention but not to limit the scope of the present invention, all the numbers used in this application to express the amount, percentage, and other numerical values should be understood as modified by the word "about" in all cases. Therefore, unless otherwise specified, the numerical parameters listed in the specification and the appended claims are approximate values, which may be changed according to the different ideal properties attempted to be obtained. Each numerical parameter should at least be regarded as obtained based on the reported significant figures and by conventional rounding methods.
[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.
[0028] The embodiment of the present invention provides a low-noise friction material, which includes the following components, measured by mass: 5-20 parts of modified phenolic resin, 2-10 parts of aramid fibers, 1-4 parts of potassium titanate whiskers, 5-15 parts of glass fibers, 3-15 parts of modified gel vermiculite, 3-7 parts of rubber powder, 15-30 parts of graphite, 2-10 parts of aluminum oxide and 20-40 parts of barium sulfate; wherein the modified gel vermiculite is prepared by mixing gel vermiculite with petroleum coke particles.
[0029] In this embodiment, the modified phenolic resin is usually cashew nut shell oil modified phenolic resin. The phenolic resin is used as a binder of the friction material to bond the components into a whole. Phenolic resin (PR) has high mechanical strength, good heat resistance and dimensional stability, cheap raw materials and easy processing. It is the most commonly used matrix resin for polymer-based friction materials. Aramid fiber and potassium titanate whisker are used in combination to reduce the hardness of the friction material while improving thermal stability and thermal decay resistance. Glass fiber is used as a reinforcing fiber to increase the strength of the friction material and thus enhance wear resistance. Rubber powder and graphite are used as lubricants to reduce the change in friction coefficient during braking. Alumina is used as an abrasive to increase the friction coefficient of the friction material. Barium sulfate is used as an inorganic filler to improve the thermal stability of the friction material and improve thermal decay. The modified gel vermiculite is a functional reinforcing filler with a porous structure having good sound absorption effect. It can be combined with other components to significantly improve the generation of friction noise of the friction material, so that the manufactured brake pad greatly reduces the braking noise and improves the braking comfort. The modified gel vermiculite is mixed with aramid fiber and other components. On the one hand, the modified gel vermiculite itself is composed of petroleum coke particles and gel vermiculite. The petroleum coke particles have a porous particle structure and good adsorption. After being mixed with the gel vermiculite, they will adhere to the pores and surface of the gel vermiculite, which has the effect of reducing the wear of the vermiculite. On the other hand, the aramid fiber has a soft texture, and its multi-branched and multi-tentacle structure can also well fill and link the modified gel vermiculite and the porous pores on the microstructure of the friction material matrix, which increases the strength and further reduces the wear, which is beneficial to maintaining the stability of the friction coefficient of the brake pad at room temperature and high temperature and reducing the wear of the friction material.
[0030] In order to better balance the improvement of noise reduction performance and anti-wear performance, preferably, the following components are included, by mass: 14 parts of modified phenolic resin, 5 parts of aramid fiber, 2 parts of potassium titanate whisker, 5 parts of glass fiber, 6 parts of modified gel vermiculite, 3 parts of rubber powder, 25 parts of graphite, 10 parts of aluminum oxide and 30 parts of barium sulfate.
[0031] The modified phenolic resin described above is cashew nut shell oil modified phenolic resin. Cashew nut shell oil modified phenolic resin can improve the interface bonding condition of inorganic fibers, filler particles such as graphite, aluminum oxide, barium sulfate, modified gel vermiculite, etc. in brake pads, thereby reducing the thermal decomposition, thermal decay and thermal cracking of brake pads, and effectively improving their wear resistance and mechanical properties.
[0032] The noise reduction effect of using gel vermiculite is better than that of vermiculite, but adding it to the friction material in the form of gel alone is likely to cause great wear of the product, thereby reducing the noise reduction performance and failing to achieve the desired effect. The present invention first generates gel on the surface of flaky vermiculite by reacting water glass and alkali, and then ages it to obtain gel vermiculite with a porous structure, which is then blended with petroleum coke particles to make the pores and surface of the gel vermiculite with a porous structure adhere to petroleum coke particles with high porosity, thereby improving the porosity of the modified gel vermiculite and obtaining a modified gel vermiculite with a rich pore structure. The density of the modified gel vermiculite prepared by the method of the present invention is 0.08-0.2g / cm 3 , melting point is 1379-1400℃, thermal conductivity is 0.04-0.06kcal / m 2 h℃, thereby achieving excellent noise reduction effect. On the other hand, the petroleum coke particles constitute the friction particles of the gel vermiculite, which improves its wear resistance and reduces the wear of the friction material. Specifically, the preparation method of the modified gel vermiculite includes:
[0033] S11, mixing water glass and flaky vermiculite in a mass ratio of 7:4;
[0034] S12, adding 1-2% of the mass of the alkali to the mixture of step S11 until gel is generated, placing the gel for aging, and then drying to obtain gel vermiculite;
[0035] S13, uniformly mixing the gel vermiculite and petroleum coke particles in a mass ratio of 7:3 to obtain the modified gel vermiculite.
[0036] Among them, step S13 uses a plowshare mixer to evenly mix the gel vermiculite and petroleum coke particles in a mass ratio of 7:3, thereby utilizing the smaller internal space of the plowshare mixer to reduce the particle diameter of the gel vermiculite, and under pressure extrusion, it is beneficial for the coke particles to evenly adhere to the gel vermiculite.
[0037] Optionally, the particle diameter of the modified gel vermiculite is 0.5-1.5 mm. A three-factor three-level orthogonal test is performed on the particle size of the modified gel vermiculite, the vermiculite content and the resin content. The level setting of each factor is shown in Table 1, and the experimental group setting and experimental results are shown in Table 2. Taking the A1B2C3 group as an example, A1 indicates that the content of the modified gel vermiculite is 35%, B2 indicates that the particle size of the modified gel vermiculite is 0.80 mm, and C3 indicates that the type of resin is selected from the high temperature resistant modified phenolic resin of cashew nut shell oil, and the content is 65%. In addition to the above three factors, the remaining components such as aramid fiber, potassium titanate whisker, etc. remain consistent. The results showed that when the particle size of the modified gel vermiculite increased from 0.56 mm to 0.80 mm, the impact strength showed an increasing trend, but when the particle size further increased from 0.80 mm to 1.25 mm, the strength decreased slightly. The particle size of 0.80 mm was the best, at which the impact strength was the largest and the impact resistance was the best. Therefore, the particle diameter of the modified gel vermiculite is preferably 0.56-1.25 mm, more preferably 0.8 mm.
[0038] Table 1 Level settings of each factor
[0039]
[0040] Table 2 Experimental group settings and experimental results
[0041] Material code Z1 Z2 Z3 Z4 Z5 Trial plan A1B2C3 A2B1C3 A2B2C3 A2B3C3 A3B2C3 Modified gel vermiculite content (%) 35 45 45 45 55 Modified gel vermiculite particle size (mm) 0.80 0.56 0.80 1.25 0.80 Cashew nut shell oil modified phenolic resin content (%) 65 55 55 55 45 <![CDATA[Impact strength J / cm 2 > 4.26 3.82 4.08 3.85 3.92
[0042] Based on the same inventive concept, another embodiment of the present invention provides a method for preparing the low-noise friction material as described above, comprising the following steps:
[0043] S21, ingredients: weigh each component according to the proportion, premix the modified gel vermiculite and aramid fiber, then add other components and mix them evenly;
[0044] S22, hot pressing: hot pressing the mixed material in step S21 to obtain a preform;
[0045] S23, post-curing treatment: after drying the preform, post-curing treatment is performed to obtain a low-noise friction material.
[0046] In this embodiment, aramid fiber and gel vermiculite are first premixed separately, and then mixed with other components. The soft texture, high strength, and high temperature resistance of aramid fiber can be utilized to make the multi-branched and multi-tentacle structure of aramid fiber fill the pores of modified gel vermiculite, and then mixed with other components. Aramid fiber acts as a link network to fix the modified gel vermiculite in the friction material matrix structure and fill the pores in the link matrix structure, thereby increasing the matrix strength, reducing the wear of the modified gel vermiculite and the matrix, and greatly improving the wear resistance at room temperature and high temperature. The preparation method of the low-noise friction material has the same advantages as the low-noise friction material described above over the prior art, and will not be repeated here.
[0047] In step S21, a plowshare mixer is used to stir and mix so that each component is fully dispersed and mixed evenly.
[0048] In step S22, the hot pressing molding operation includes: a molding temperature of 160°C, a pre-pressing time of 10s, a pressure relief and exhaust time of 5s, a pressure relief and exhaust number of 5 times, a hot pressing pressure of 10MPa, and a pressing time of 10min.
[0049] In step S23, the post-curing treatment operation includes: keeping the temperature at 160°C for 10 hours.
[0050] Based on the same inventive concept, another embodiment of the present invention provides the use of the low-noise friction material as described above in the preparation of brake pads or brake shoes.
[0051] The application of the low-noise friction material in the preparation of brake pads or brake shoes has the same advantages as the low-noise friction material described above over the prior art, which will not be repeated here.
[0052] The present invention is further described below in conjunction with specific examples. The experimental methods in the following examples without specifying specific conditions are generally carried out according to the conditions recommended by the manufacturer.
[0053] Example 1
[0054] A method for preparing a low-noise friction material comprises the following steps:
[0055] S21, ingredients: weigh each component in proportion, among which, 14 parts of cashew nut shell oil modified phenolic resin, 5 parts of aramid fiber, 2 parts of potassium titanate whisker, 5 parts of glass fiber, 6 parts of modified gel vermiculite, 3 parts of rubber powder, 25 parts of graphite, 10 parts of alumina, 30 parts of barium sulfate, premix the modified gel vermiculite and aramid fiber to achieve full mixing, then add the remaining components, stir and mix them with a plowshare mixer to fully disperse the various materials and mix them evenly;
[0056] S22, hot pressing molding: putting the mixed material of step S21 into a four-column hydraulic press for hot pressing molding, the molding temperature is 160° C., the pre-pressing time is 10 s, the pressure relief and exhaust time is 5 s, the pressure relief and exhaust times are 5 times, the hot pressing pressure is 10 MPa, and the pressing time is 10 min to obtain a preform;
[0057] S23, post-curing treatment: after drying the preform, place it in an electric constant temperature blast drying oven, keep it at 160°C for 10 hours, and then perform curing treatment to obtain a low-noise friction material.
[0058] The preparation method of the modified gel vermiculite used above comprises the following steps:
[0059] S11, mixing water glass and flaky vermiculite in a mass ratio of 7:4;
[0060] S12, adding 2% of the mass of the alkali to the mixture of step S11 until gel is generated, placing the gel for aging, and then drying to obtain gel vermiculite;
[0061] S13, adding gel vermiculite and petroleum coke particles in a mass ratio of 7:3 into a plowshare mixer, mixing them, and obtaining modified gel vermiculite with a particle diameter of 0.8 mm.
[0062] Example 2
[0063] A method for preparing a low-noise friction material comprises the following steps:
[0064] S21, ingredients: weigh each component in proportion, among which, 14 parts of cashew nut shell oil modified phenolic resin, 5 parts of aramid fiber, 2 parts of potassium titanate whisker, 5 parts of glass fiber, 5 parts of modified gel vermiculite, 3 parts of rubber powder, 25 parts of graphite, 10 parts of alumina, 31 parts of barium sulfate, premix the modified gel vermiculite and aramid fiber to achieve full mixing, then add the remaining components, use a plowshare mixer to stir and mix, so that various materials are fully dispersed and mixed evenly;
[0065] S22, hot pressing molding: putting the mixed material of step S21 into a four-column hydraulic press for hot pressing molding, the molding temperature is 160° C., the pre-pressing time is 10 s, the pressure relief and exhaust time is 5 s, the pressure relief and exhaust times are 5 times, the hot pressing pressure is 10 MPa, and the pressing time is 10 min to obtain a preform;
[0066] S23, post-curing treatment: after drying the preform, place it in an electric constant temperature blast drying oven, keep it at 160°C for 10 hours, and then perform curing treatment to obtain a low-noise friction material.
[0067] The preparation method of the modified gel vermiculite used above is the same as that in Example 1.
[0068] Example 3
[0069] A method for preparing a low-noise friction material comprises the following steps:
[0070] S21, ingredients: weigh each component in proportion, among which, 14 parts of cashew nut shell oil modified phenolic resin, 5 parts of aramid fiber, 2 parts of potassium titanate whisker, 5 parts of glass fiber, 7 parts of modified gel vermiculite, 3 parts of rubber powder, 25 parts of graphite, 10 parts of alumina, 29 parts of barium sulfate, premix the modified gel vermiculite and aramid fiber to achieve full mixing, then add the remaining components, stir and mix them with a plowshare mixer to fully disperse the various materials and mix them evenly;
[0071] S22, hot pressing molding: putting the mixed material of step S21 into a four-column hydraulic press for hot pressing molding, the molding temperature is 160° C., the pre-pressing time is 10 s, the pressure relief and exhaust time is 5 s, the pressure relief and exhaust times are 5 times, the hot pressing pressure is 10 MPa, and the pressing time is 10 min to obtain a preform;
[0072] S23, post-curing treatment: after drying the preform, place it in an electric constant temperature blast drying oven, keep it at 160°C for 10 hours, and then perform curing treatment to obtain a low-noise friction material.
[0073] The preparation method of the modified gel vermiculite used above is the same as that in Example 1.
[0074] Comparative Example 1
[0075] Comparative Example 1 is substantially the same as Example 1, except that the modified gel vermiculite in Example 1 is replaced by ordinary vermiculite purchased from Hebei Bonite with the item number F-11. The remaining operations are the same as those in Example 1.
[0076] Comparative Example 2
[0077] Comparative Example 2 is basically the same as Example 1, except that the petroleum coke particles in the modified gel vermiculite in Example 1 are replaced with carbon fibers (purchased from Hebei Bonite, item number F-11) to obtain modified gel vermiculite blended with carbon fibers and gel vermiculite, and the remaining operations are the same as Example 1.
[0078] Low noise friction material performance test
[0079] The friction properties of the friction materials prepared in Examples 1-3 and Comparative Examples 1-2 were measured at different temperatures on a constant speed friction tester, and the results are shown in Table 3. The wear properties at different temperatures were then measured using a constant speed friction tester, and the results are shown in Table 4. The noise of the friction material was further tested using a scaled bench friction tester, with the base noise set to 72 dB, and the results are shown in Table 5.
[0080] Table 3 Comparative test results of friction properties of friction materials prepared in Examples 1-3 and Comparative Examples 1-2
[0081]
[0082] Table 4 Comparative test results of wear performance of friction materials prepared in Examples 1-3 and Comparative Examples 1-2
[0083]
[0084] Table 5 Comparative test results of friction properties of friction materials prepared in Examples 1-3 and Comparative Examples 1-2
[0085]
[0086] As shown in Table 3-5, the friction material prepared in Example 1-3 has a more stable friction coefficient at high temperature, a significantly reduced wear rate, and a more excellent noise reduction performance than the friction material prepared in Example 1-2 using different methods of preparing ordinary vermiculite or modified gel vermiculite. Moreover, by adjusting the content of modified gel vermiculite, it is found that when 6 parts, 5 parts, and 7 parts of modified gel vermiculite are added to Examples 1-3, respectively, the friction coefficient of the friction material prepared in Example 2 is the most stable. The wear degree of each example is similar below 250°C, but Example 2 is better in the high-temperature wear stage above 250°C, but all are better than Comparative Examples 1-2. This shows that the addition of the modified gel vermiculite of the present invention effectively improves the noise of the friction material, while also taking into account the reduction of the wear of the friction material, improving its anti-wear performance at high temperature and ensuring the stability of the friction coefficient at high temperature, which will be beneficial to its application in the field of brake pads and / or brake pads, and improve the performance of brake pads and / or brake pads.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A low-noise friction material, characterized in that: The invention comprises the following components by weight: 5-20 parts of cashew nut shell oil modified phenolic resin, 2-10 parts of aramid fiber, 1-4 parts of potassium titanate whisker, 5-15 parts of glass fiber, 3-15 parts of modified gel vermiculite, 3-7 parts of rubber powder, 15-30 parts of graphite, 2-10 parts of aluminum oxide and 20-40 parts of barium sulfate; Wherein, the preparation method of the modified gel vermiculite comprises: S11, mixing water glass and flaky vermiculite in a mass ratio of 7:4; S12, adding 1-2% of the mass of the alkali to the mixture of step S11 until a gel is generated, placing the gel for aging, and then drying to obtain gel vermiculite; S13, uniformly mixing the gel vermiculite and petroleum coke particles in a mass ratio of 7:3 to obtain the modified gel vermiculite.
2. The low-noise friction material according to claim 1, characterized in that: The invention comprises the following components by weight: 14 parts of cashew nut shell oil modified phenolic resin, 5 parts of aramid fiber, 2 parts of potassium titanate whisker, 5 parts of glass fiber, 6 parts of modified gel vermiculite, 3 parts of rubber powder, 25 parts of graphite, 10 parts of aluminum oxide and 30 parts of barium sulfate.
3. The low noise friction material according to claim 1, characterized in that: The modified gel vermiculite has a density of 0.08-0.2 g / cm³, a melting point of 1379-1400°C, and a thermal conductivity of 0.04-0.06 kcal / m²h°C.
4. The low-noise friction material according to claim 1, characterized in that: The particle diameter of the modified gel vermiculite is 0.8 mm.
5. A method for preparing a low-noise friction material, characterized in that: The method for preparing the low-noise friction material according to any one of claims 1 to 4 comprises the following steps: S21, ingredients: weigh each component according to the proportion, premix the modified gel vermiculite and aramid fiber, then add other components and mix them evenly; S22, hot pressing: hot pressing the mixed material in step S21 to obtain a preform; S23, post-curing treatment: after drying the preform, post-curing treatment is performed to obtain a low-noise friction material.
6. The method for preparing a low-noise friction material according to claim 5, characterized in that: In step S22, the hot pressing molding operation includes: a molding temperature of 160°C, a pre-pressing time of 10s, a pressure relief and exhaust time of 5s, a pressure relief and exhaust number of 5 times, a hot pressing pressure of 10MPa, and a pressing time of 10min.
7. The method for preparing a low-noise friction material according to claim 5, characterized in that: In step S23, the post-curing treatment operation includes: keeping the temperature at 160°C for 10 hours.
8. Use of the low-noise friction material according to any one of claims 1 to 4 in the preparation of brake pads or brake shoes.