A particle reinforced high-strength bainite medium-temperature forging steel and preparation method thereof
The preparation method of particle-reinforced high-strength bainitic medium-temperature forged steel, combined with Ti-V composite microalloying technology and controlled forging and controlled cooling process, solves the problem of long bainitic phase transformation time and inability to balance performance, and significantly improves the performance of the steel. Excellent mechanical properties, achieving efficient industrial production.
Patent Information
- Application Number
- CN202211349425.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-31
AI Technical Summary
The long bainite phase transformation time in the existing technology limits the industrial production of high-strength bainite steel. At the same time, it is difficult for the existing process to take into account the high performance and wear resistance of the steel.
The preparation method of particle-reinforced high-strength bainitic medium-temperature forged steel is adopted. Through the process flow of hot forging, medium-temperature forging, insulation and tempering treatment, Ti-V composite micro-alloying technology and controlled forging and controlled cooling process are used to shorten the bainite. phase transformation time to improve the mechanical properties of steel.
Significantly shortened the bainite phase transformation time, improved the tensile strength, yield strength and elongation of the steel to 1400~1600MPa, 1200~1400MPa and 10~15%, and improved the steel through fine grain strengthening and precipitation strengthening mechanisms. comprehensive mechanical properties.
Smart Images

Figure CN115976310B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material preparation, and in particular to a particle-reinforced high-strength bainite medium-temperature forging steel and a preparation method thereof. Background Art
[0002] In recent decades, the development and application of high-strength wear-resistant steel plates have developed rapidly. This type of steel is developed on the basis of low-alloy high strength, with good wear resistance and service life up to several times that of traditional structural steel plates. High-strength wear-resistant steel plates are widely used in mining, coal, construction, ports, electricity and metallurgy machinery products with particularly harsh working conditions and high strength and high wear resistance. Such as bulldozers, loaders, excavators, dump trucks and various mining machinery, grabs, stackers, conveyor bending structures, etc. Among them, bainitic high-strength wear-resistant steel has attracted great attention from material researchers and enterprises in the field of mechanical manufacturing due to its high strength, toughness, excellent wear resistance and rolling contact fatigue resistance. At present, a complex phase structure composed of nano-scale bainitic ferrite laths and carbon-rich film-like retained austenite is prepared by low-temperature isothermal quenching process. The preparation process is simple and has good strength-plasticity matching, which has attracted widespread attention from many scholars and industrial circles at home and abroad. However, the characteristics of low-temperature transformation make the process time-consuming and lengthy, and the phase transformation takes up to dozens of hours to complete, which restricts its large-scale production and application. Therefore, shortening the austempering time and accelerating the phase transformation process of bainite are the keys to solving the industrial production of high-strength bainitic steel.
[0003] In order to accelerate the phase transformation process of bainite and obtain high-strength bainite steel, Chinese invention patent CN200810021697.5 discloses a carbide-free bainite wear-resistant steel plate and its production process, the production process is: heating the continuous casting plate; carrying out controlled rolling and controlled cold rolling on the heated continuous casting slab; after rolling, performing medium and low temperature tempering treatment on the rolled steel plate. The above process can not only simplify the production process, but also improve product performance and product quality, and obtain high-strength and high-toughness bainite wear-resistant steel. However, the hardness of its product is not high enough, which will seriously affect the wear resistance of the product, and its Si content is high, which may cause the steel to crack during rolling; Chinese invention patent CN201811347357.1 discloses a fast phase change nano-bainite steel and its preparation method, which can control the phase change time of nano-bainite within 60 minutes, significantly shorten the preparation time, and improve production efficiency, but the mechanical properties of the prepared nano-bainite steel are not high; Chinese invention patent CN200610134087.7 discloses a high-performance low-carbon bainite structural steel and its production method, which adopts the TMCP+RPC process to obtain bainite structure without modulation, has high strength, high toughness, and good welding and wear resistance, but its preparation process is relatively complicated, which is not conducive to industrial production. Summary of the invention
[0004] The present invention aims to provide a particle reinforced high-strength bainite medium-temperature forging steel and a preparation method thereof, so as to solve the problem in the prior art that the bainite phase transformation time and the performance of the obtained bainite steel cannot be taken into account at the same time.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] A method for preparing particle-reinforced high-strength bainite medium-temperature forging steel comprises the following steps:
[0007] S1. Hot forging: The steel ingot is heated to 1180-1280°C at a heating rate lower than 80°C / h for homogenization treatment, then cooled to 1180-1100°C for hot forging;
[0008] S2, medium temperature forging: cooling the hot forged steel billet obtained in step S1 to 800-650°C and performing medium temperature forging;
[0009] S3, heat preservation; the medium temperature forged steel plate obtained in step S2 is immediately placed in 300-450°C for heat preservation for 0.5-5h to complete the bainite isothermal phase transformation, and then air-cooled to room temperature;
[0010] S4, tempering treatment: the forged steel obtained in step S3 is heated to 200°C-300°C and kept at this temperature for 1-5 hours for tempering treatment, and then air-cooled to room temperature.
[0011] The principle and advantages of this scheme are: this method completely austenitizes the steel and then homogenizes it, and then hot forging at a slightly lower temperature can promote multiple recrystallization of austenite, fully refine the austenite grains, and eliminate some casting defects; and directly use the waste heat of the hot forging plate for medium-temperature forging, without the need for secondary heating, saving energy; medium-temperature forging stores a large amount of distortion energy, increases the nucleation rate and growth rate of nano-bainite during the low-temperature isothermal process, and significantly shortens the time of bainite phase transformation, so that a large amount of bainite structure can be obtained by only keeping it at 300-450℃ for 0.5-5h. And this scheme makes a large number of submicron-level precipitates dispersed in the steel obtained, and uses the fine grain strengthening and precipitation strengthening mechanism to greatly improve the comprehensive mechanical properties of the steel.
[0012] In addition, the method is feasible to operate and has high production efficiency. The invention abandons the conventional low-temperature isothermal quenching process which is both energy-consuming and time-consuming, and can be used for large-scale industrial production.
[0013] Preferably, as an improvement, in the hot forging of step S1, the total deformation of the hot forging is 60-80%, and the final forging temperature of the hot forging is not less than 850°C.
[0014] Preferably, as an improvement, in the medium-temperature forging in step S2, the total deformation of the medium-temperature forging is 40-60%, and the final forging temperature of the medium-temperature forging is not less than 500°C.
[0015] Preferably, as an improvement, in the hot forging of step S1, the steel ingot is heated to 1180-1280°C at a heating rate of 65-80°C / h for homogenization treatment.
[0016] Preferably, as an improvement, in the tempering treatment of step S4, the forged steel obtained in step S3 is heated to 200°C-300°C at a heating rate of 65-80°C / h and kept at that temperature for 1-5h for tempering treatment, and then air-cooled to room temperature.
[0017] The present invention also provides a particle-reinforced high-strength bainite medium-temperature forged steel, which is used in the preparation method of the particle-reinforced high-strength bainite medium-temperature forged steel, comprising the following elements in mass percentage: C: 0.25-0.35%, Si: 1.42-1.65%, Mn: 1.45-1.95%, Cr: 1.80-2.50%, Ni: 0.82-1.35%, Cu: 0.20-0.45%, Ti: 0.28-0.52%, V: 0.05-0.15%, and the rest is Fe and unavoidable impurities. This scheme makes the CCT curve of the steel shift to the right as a whole, and at the same time makes the pearlite transformation zone more to the right than the bainite transformation zone; so that the martensitic transformation temperature of the alloy steel obtained is 195-280°C.
[0018] Preferably, as an improvement, when the preparation method of particle reinforced high-strength bainite medium-temperature forging steel is adopted, the holding time in step S3 is 0.5-2h.
[0019] Preferably, as an improvement, when the preparation method of particle reinforced high-strength bainite medium-temperature forging steel is adopted, the holding time of the tempering treatment in step S4 is 1-2 hours.
[0020] The present invention adopts Ti-V composite microalloying technology combined with a matching controlled forging and controlled cooling process technology to prepare high-strength bainite forged steel. In the present invention, the steel blank after high-temperature homogenization is hot forged in a single-phase austenite region. A large amount of deformation energy can promote repeated recrystallization of austenite grains, refine the austenite grain structure, and eliminate some casting defects, making the steel structure denser. Through the special alloy composition design, the CCT curve is generally shifted to the right, and the pearlite transformation zone is further to the right than the bainite transformation zone, so as to ensure that it is still in the austenite single-phase region during the medium-temperature forging process and no pearlite phase transformation occurs. Under medium-temperature forging, a large number of crystal defects are generated in the steel through deformation, the nucleation rate of VC is increased, the dislocation density in the steel is significantly increased, the core of the bainite phase deformation nucleus is increased, the growth of bainite after nucleation is provided with power, and the phase transformation time of bainite at low temperature isothermal is greatly shortened (the phase transformation time is only 0.5-2h); immediately after the medium-temperature forging is completed, the forged steel plate is placed in 300-450℃ for insulation and then air-cooled to room temperature to obtain high-strength nano-bainite high-strength steel, and finally the forged steel is tempered. Since a large number of crystal defects are generated in the steel due to the medium-temperature forging, the dispersed submicron carbides in the steel can be precipitated, thereby significantly enhancing the precipitation strengthening effect of the steel and improving the fine grain strengthening increment and precipitation strengthening increment of the steel.
[0021] In summary, the present invention uses a simple controlled forging and controlled cooling process to enable high-strength steel to obtain a large amount of nano-bainite structure (large volume) in a short period of time with insulation of no more than 2 hours, and after the present invention, a large amount of submicron VC precipitates are dispersed in the steel (because the submicron carbide particles are extremely small, so even if the volume share is not large, the number can be large), and the comprehensive mechanical properties of the steel are significantly improved by using fine grain strengthening, precipitation strengthening, and solid solution strengthening mechanisms, so that the tensile strength of the steel reaches 1400-1600MPa, the yield strength reaches 1200-1400MPa, and the elongation reaches 10-15%. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a process flow chart of the present invention.
[0023] Figure 2 This is the CCT diagram of Example 1 of the present invention.
[0024] Figure 3 This is the metallographic structure diagram of Example 1 of the present invention.
[0025] Figure 4 This is the SEM image of Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The following is further described in detail through specific implementation methods:
[0027] A particle reinforced high-strength bainite medium-temperature forging steel comprises the following elements in percentage by mass: C: 0.25-0.35%, Si: 1.42-1.65%, Mn: 1.45-1.95%, Cr: 1.80-2.50%, Ni: 0.82-1.35%, Cu: 0.20-0.45%, Ti: 0.28-0.52%, V: 0.05-0.15%, and the rest is Fe and inevitable impurities.
[0028] Combination Figure 1 A method for preparing a particle-reinforced high-strength bainite medium-temperature forging steel comprises the following steps:
[0029] (1) Melting and Casting: Take the steel containing the above ingredients, melt it in a vacuum induction furnace and cast it into a steel ingot.
[0030] (2) Hot forging: The steel ingot is heated to 1180-1280°C at a heating rate of 65-80°C / h and homogenized for 1.5-2h, then cooled to 1180-1100°C at a cooling rate of 10°C / s for hot forging; the total deformation of hot forging is 60-80%, and the final forging temperature is not less than 850°C.
[0031] (3) Medium temperature forging: The hot forged blank obtained by the above hot forging is cooled to 800-650°C at a cooling rate of 10°C / s and then subjected to medium temperature forging; the total deformation of the medium temperature forging is 40-60%, and the final forging temperature of the medium temperature forging is not less than 500°C.
[0032] (4) Insulation: The steel plate obtained by medium temperature forging is immediately placed in a 300-450°C salt bath furnace for insulation for 0.5-2h to complete the isothermal phase transformation of bainite, and then air-cooled to room temperature.
[0033] (5) Tempering treatment: The forged steel is heated to 200-300°C at a heating rate of 65-80°C / h and kept at this temperature for 1-2h, and then air-cooled to room temperature to obtain a high-strength bainite forged steel.
[0034] In order to verify the present invention, the following specific examples and comparative examples are provided.
[0035] Example 1
[0036] A particle-reinforced high-strength bainite medium-temperature forging steel comprises the following elements in percentage by mass: C: 0.28%, Si: 1.52%, Mn: 1.65%, Cr: 2.00%, Ni: 1.16%, Cu: 0.36%, Ti: 0.34%, V: 0.12%, and the remainder is Fe and unavoidable impurities. A method for preparing a particle-reinforced high-strength bainite medium-temperature forging steel comprises the following steps:
[0037] (1) Melting and Casting: Take the steel containing the above ingredients, melt it in a vacuum induction furnace and cast it into a steel ingot.
[0038] (2) Hot forging: The steel ingot was heated to 1250°C at a heating rate of 70°C / h and homogenized for 2h, then cooled to 1180°C at a cooling rate of 10°C / s for hot forging; the start forging temperature was 1120°C, the total hot forging deformation was 70%, and the final forging temperature was 950°C.
[0039] (3) Medium-temperature forging: The hot forged blank obtained by the above hot forging is cooled to 800°C at a cooling rate of 10°C / s and then subjected to medium-temperature forging; the start forging temperature is 750°C, the total deformation of the medium-temperature forging is 50%, and the final forging temperature is 550°C.
[0040] (4) Insulation: The steel plate obtained by medium temperature forging was immediately placed in a 350°C salt bath furnace for 2 h to complete the isothermal phase transformation of bainite, and then air-cooled to room temperature.
[0041] (5) Tempering treatment: The forged steel was heated to 250°C at a heating rate of 70°C / h and kept at that temperature for 2h, and then air-cooled to room temperature to obtain a high-strength bainite forged steel.
[0042] Example 2
[0043] A particle-reinforced high-strength bainite medium-temperature forging steel comprises the following elements in percentage by mass: C: 0.25%, Si: 1.45%, Mn: 1.48%, Cr: 1.82%, Ni: 0.94%, Cu: 0.35%, Ti: 0.36%, V: 0.08%, and the remainder is Fe and unavoidable impurities. The preparation method comprises:
[0044] (1) Melting and casting: According to the design requirements of steel components, the steel is melted and cast into steel ingots in a vacuum induction furnace;
[0045] (2) Hot forging: The steel ingot was heated to 1250°C at a heating rate of 65°C / h and homogenized for 2h, then cooled to 1250°C at a cooling rate of 10°C / s for hot forging; the start forging temperature was 1150°C, the total hot forging deformation was 70%, and the final forging temperature was 970°C.
[0046] (3) Medium-temperature forging: The hot forged blank obtained by the above hot forging is cooled to 800°C at a cooling rate of 10°C / s and then subjected to medium-temperature forging; the start forging temperature is 750°C, the total deformation of the medium-temperature forging is 50%, and the final forging temperature is 570°C.
[0047] (4) Insulation: The forged steel plate forged at medium temperature is immediately placed in a 400°C salt bath furnace for 2 hours to complete the isothermal phase transformation of bainite, and then air-cooled to room temperature.
[0048] (5) Tempering treatment: The forged steel was heated to 280°C at a heating rate of 65°C / h and kept at that temperature for 2h, and then air-cooled to room temperature to obtain a high-strength bainite forged steel.
[0049] Example 3
[0050] A particle-reinforced high-strength bainite medium-temperature forging steel comprises the following elements in percentage by mass: C: 0.30%, Si: 1.53%, Mn: 1.62%, Cr: 2.21%, Ni: 1.18%, Cu: 0.36%, Ti: 0.28%, V: 0.15%, and the remainder is Fe and unavoidable impurities. The preparation method comprises:
[0051] (1) Melting and casting: According to the design requirements of steel components, the steel is melted and cast into steel ingots in a vacuum induction furnace;
[0052] (2) Hot forging: The steel ingot was heated to 1250°C at a heating rate of 75°C / h and homogenized for 2h, then cooled to 1150°C at a cooling rate of 10°C / s for hot forging; the start forging temperature was 1120°C, the total hot forging deformation was 70%, and the final forging temperature was 900°C.
[0053] (3) Medium-temperature forging: The hot forged blank obtained by the above hot forging is cooled to 800°C at a cooling rate of 10°C / s and then subjected to medium-temperature forging; the start forging temperature is 730°C, the total deformation of the medium-temperature forging is 50%, and the final forging temperature is 520°C.
[0054] (4) Insulation: The steel plate obtained by medium temperature forging was immediately placed in a 300°C salt bath furnace for 2 h to complete the isothermal phase transformation of bainite, and then air-cooled to room temperature.
[0055] (5) Tempering treatment: The forged steel was heated to 230°C at a heating rate of 75°C / h and kept at that temperature for 2h, and then air-cooled to room temperature to obtain a high-strength bainite medium-temperature forged steel.
[0056] Comparative Example 1
[0057] Comparative Example 1 of the present invention is a commercial nano-bainite steel on the market, and its chemical composition by mass percentage is: C: 0.25%, Si: 0.6%, Mn: 1.7%, Cr: 0.5%, Ni: 1.1%, V: 0.13%, and the rest is Fe and unavoidable impurities.
[0058] The preparation method is exactly the same as that in Example 1.
[0059] Comparative Example 2
[0060] Comparative Example 2 of the present invention has the same chemical composition as Example 1, and the preparation method comprises:
[0061] (1) Hot forging: The steel ingot was heated to 1250°C at a heating rate of 70°C / h and homogenized for 2h, then cooled to 1180°C at a cooling rate of 10°C / s for hot forging; the start forging temperature was 1120°C, the total hot forging deformation was 70%, and the final forging temperature was 950°C.
[0062] (2) Insulation: The hot forged steel plate is immediately placed in a 350°C salt bath furnace for 2 h to undergo isothermal bainite transformation, and then air-cooled to room temperature.
[0063] (3) Tempering treatment: The forged steel was heated to 250°C at a heating rate of 70°C / h and kept at that temperature for 2h, and then air-cooled to room temperature to obtain bainitic forged steel.
[0064] Comparative Example 3
[0065] Comparative Example 3 of the present invention has the same chemical composition as Example 1, and the preparation method comprises:
[0066] (1) Hot forging: The steel ingot was heated to 1250°C at a heating rate of 70°C / h and homogenized for 2h, then cooled to 1180°C at a cooling rate of 10°C / s for hot forging; the start forging temperature was 1120°C, the total hot forging deformation was 70%, and the final forging temperature was 950°C.
[0067] (2) Insulation: The hot forged steel plate is immediately placed in a 350°C salt bath furnace for 8 hours to undergo isothermal bainite transformation, and then air-cooled to room temperature.
[0068] (3) Tempering treatment: The forged steel was heated to 250°C at a heating rate of 70°C / h and kept at that temperature for 2h, and then air-cooled to room temperature to obtain bainitic forged steel.
[0069] The high-strength bainite medium-temperature forging steel prepared in Examples 1-3 of the present invention has a microstructure of fine and uniform bainite and a very small amount of martensite, and a large number of submicron carbides are dispersed in the matrix, so that the high-strength bainite steel has a high surface hardness and yield strength, while also ensuring sufficient impact toughness. The high-strength bainite medium-temperature forging steel prepared in Example 1 is used as an example for detailed description:
[0070] Figure 2 In order to implement the CCT diagram of Case 1, through special chemical composition design, the pearlite transformation zone and the ferrite transformation zone are further to the right than the bainite transformation zone, ensuring that the medium-temperature forging process is still in the austenite single-phase region without other phase changes. In this way, the lattice distortion and deformation energy storage generated by medium-temperature forging can promote the rapid transformation of bainite in the subsequent isothermal process in the bainite transformation temperature zone, significantly shortening the bainite transformation time.
[0071] Figure 3This is the metallographic structure diagram of Example 1. It can be seen from the figure that its structure is composed of nano-bainite, film-like residual austenite and a small amount of martensite. Among them, the bainite grains are fine and uniform. From the fine grains, it can be inferred that fine grain strengthening has made a significant contribution to the improvement of yield strength.
[0072] Figure 4 This is the SEM image of Example 1. It can be seen from the figure that there are many dispersed submicron precipitates in the matrix structure. The shape of the precipitates is mainly square or circular. The submicron precipitates can improve the strength of high-strength steel by hindering dislocation movement.
[0073] Table 1 shows the microstructure results of Examples 1-3 and Comparative Examples 1-3. It can be seen from Table 1 that the microstructures of Examples 1-3 are a large amount of bainite + a small amount of martensite + a trace amount of submicron-sized particle carbide, and the volume fraction of bainite is above 92%; the microstructure of Comparative Example 1 is a mixed structure of bainite, pearlite and martensite, and the volume fraction of bainite is only 60%. This is because the chemical composition of the embodiments is specially designed, and the commercial bainitic steel on the market will undergo other phase changes during the medium-temperature forging process; the chemical compositions of Comparative Examples 2 and 3 are exactly the same as those of Example 1, but neither of them is subjected to medium-temperature forging treatment. Comparative Example 2 is kept warm in the bainite transformation temperature zone for 2 hours, and Comparative Example 3 is kept warm for 8 hours. It can be seen from Table 1 that if Example 1 is not subjected to medium-temperature forging treatment, and is directly isothermal after hot forging, it takes 8 hours of isothermal treatment to barely reach the bainite content after medium-temperature forging treatment.
[0074] Table 1 Microstructure of Examples 1-3 and Comparative Examples 1-3
[0075] Sample No. Microstructure Implementation Case 1 Bainite about 95% + martensite about 5% + trace submicron particle carbide Implementation Case 2 Bainite about 92% + martensite about 8% + trace submicron particle carbide Implementation Case 3 Bainite about 93% + martensite about 7% + trace submicron particle carbide Comparative Case 1 Bainite 60% + pearlite 30% + martensite 10% Comparative Case 2 Bainite 62% + Martensite 38% Comparative Case 3 Bainite 89% + Martensite 11%
[0076] Table 2 Mechanical properties of Examples 1-3 and Comparative Examples 1-3
[0077] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Yield strength, MPa 1310 1290 1360 980 1080 1280 Tensile strength, MPa 1540 1500 1480 1120 1210 1480 Elongation, % 12 14 10 8 9 12 Impact energy (room temperature), J 35 36 32 26 23 32 Surface hardness, HB 476 452 460 386 492 468
[0078] Table 2 shows the mechanical property results of Examples 1-3 and Comparative Examples 1-3. It can be seen from Table 2 that the yield strength and tensile strength of Examples 1-3 are higher than those of Comparative Examples 1-3; Comparative Example 1 has the lowest mechanical properties, mainly because pearlite transformation occurs during the medium-temperature forging stage, which affects its mechanical properties, and the chemical composition of Comparative Example 1 determines that the number of carbides is small, and the precipitation strengthening increment must be less than that of Examples 1-3; Comparative Examples 2-3 are not subjected to medium-temperature forging treatment, and their bainite content is lower than that of the embodiments.
[0079] In summary, the present invention aims to obtain a high-strength bainitic forged steel, which adopts a special composition design and combines the controlled forging and controlled cooling process to introduce the medium-temperature forging process into the preparation of bainitic steel, significantly reduce the transformation time of bainite, improve the production efficiency of nano-bainitic steel, and significantly improve the comprehensive mechanical properties of the steel, so that the tensile strength of the steel reaches 1400-1600MPa, the yield strength reaches 1200-1400MPa, and the elongation reaches 10-15%.
[0080] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for preparing particle-reinforced high-strength bainite medium-temperature forging steel, characterized in that: The following steps are involved: S1. Hot forging: the steel ingot is heated to 1180-1280°C at a heating rate lower than 80°C / h for homogenization treatment, then cooled to 1180-1100°C for hot forging; wherein the steel ingot comprises the following elements in mass percentage: C: 0.25-0.35%, Si: 1.42-1.65%, Mn: 1.45-1.95%, Cr: 1.80-2.50%, Ni: 0.82-1.35%, Cu: 0.20-0.45%, Ti: 0.28-0.52%, V: 0.05-0.15%, and the rest is Fe and unavoidable impurities; S2, medium temperature forging: cooling the hot forged steel billet obtained in step S1 to 800-650°C and performing medium temperature forging; S3, heat preservation; the medium temperature forged steel plate obtained in step S2 is immediately placed in 300-450°C for heat preservation for 0.5-5h to complete the bainite isothermal phase transformation, and then air-cooled to room temperature; S4, tempering treatment: the forged steel obtained in step S3 is heated to 200°C-300°C and kept at this temperature for 1-5 hours for tempering treatment, and then air-cooled to room temperature.
2. The method for preparing particle reinforced high-strength bainite medium-temperature forging steel according to claim 1, characterized in that: In the hot forging of step S1, the total deformation of hot forging is 60-80%, and the final forging temperature of hot forging is not less than 850°C.
3. The method for preparing particle reinforced high-strength bainite medium-temperature forging steel according to claim 1, characterized in that: In the medium temperature forging in step S2, the total deformation of the medium temperature forging is 40-60%, and the final forging temperature of the medium temperature forging is not less than 500°C.
4. The method for preparing the particle reinforced high-strength bainite medium-temperature forging steel according to claim 1, characterized in that: In the hot forging of step S1, the steel ingot is heated to 1180-1280° C. at a heating rate of 65-80° C. / h for homogenization treatment.
5. The method for preparing particle reinforced high-strength bainite medium-temperature forging steel according to claim 1, characterized in that: In the tempering treatment of step S4, the forged steel obtained in step S3 is heated to 200°C-300°C at a heating rate of 65-80°C / h and kept at that temperature for 1-5h for tempering treatment, and then air-cooled to room temperature.
6. The method for preparing particle reinforced high-strength bainite medium-temperature forging steel according to claim 1, characterized in that: The insulation time in step S3 is 0.5-2h.
7. The method for preparing particle reinforced high-strength bainite medium-temperature forging steel according to claim 1, characterized in that: The holding time of the tempering treatment in step S4 is 1-2h.
Citation Information
Patent Citations
High-performance low-carbon bainite construction steel and producing method thereof
CN101168826A
Carbides-free bainite wear resistant steel plate and production process thereof
CN101338399A
Rapid phase change nanometer bainite steel and preparation method
CN109295389A
Steel products and process for production thereof
CN101952471A
Method for manufacturing high-strength cold-rolled / hot-rolled trip steel having a tensile strength of 590 mpa grade, superior workability, and low mechanical-property deviation
CN103249847A