A crystal material and its preparation method and application

Through the new crystal material 4 (C3N6H6)·HPF6·4H2O, the existing birefringence crystals have been solved in the UV deep ultraviolet band, and the good transmittance in the range of 200nm to 2500nm and Large birefringence, suitable for optical components, and is stable and easy to process and grow at high temperatures.

CN115976646BActive Publication Date: 2024-11-12FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211085709.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-06
Publication Date
2024-11-12
Estimated Expiration
2042-09-06

AI Technical Summary

Technical Problem

The existing birefringence crystals have insufficient transmission capacity in the ultraviolet deep ultraviolet band and have a small birefringence, which limits their application in the field of optical, especially in high temperatures, and are difficult to obtain. Size single crystal.

Method used

Using a new crystal material 4 (C3N6H6)·HPF6·4H2O, it was shown through first principle calculation that it has a large birefringence at 1042nm, and was prepared by aqueous solution method, adjusting the pH value and controlling the reaction conditions to obtain Single crystal structure with good transmittance.

Benefits of technology

The crystal material has good transmittance and a large birefringence in the range of 200 nm to 2500 nm. It is suitable for polarized beam splitting prisms and optical components, and has good stability at high temperatures and is easy to process and grow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115976646B_ABST
    Figure CN115976646B_ABST
Patent Text Reader

Abstract

The present application discloses a crystal material and its preparation method and application, which belongs to the field of optical materials. A crystal material, the chemical formula of which is 4(C3N6H6)·HPF6·4H2O; C3N6H6 is connected by hydrogen bonds of N‑H···N in the molecule; (PF6) ‑ It forms a three-dimensional structure with C3N6H6 through intramolecular hydrogen bonds. The first principle calculation shows that the crystal has a large birefringence. The birefringence at 1042nm is 0.241; the birefringent crystal material has good transmittance in a wide spectrum range of 200nm to 2500nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a crystal material and a preparation method and application thereof, belonging to the field of optical materials. Background Art

[0002] When a beam of light is irradiated on the crystal interface, two beams of refracted light will be generated. This phenomenon is called birefringence. The reason for the birefringence is due to the anisotropy of the crystal material itself. Crystals that can produce this phenomenon are called birefringent crystals. Crystals that can produce birefringence can be divided into uniaxial crystals and biaxial crystals. Crystals with trigonal, tetragonal or hexagonal crystal systems are uniaxial crystals, and crystals with orthorhombic, monoclinic and triclinic crystal systems are called biaxial crystals. Birefringent crystals are widely used in the field of optics, such as photolithography, communications and micromachining.

[0003] At present, the birefringent crystals that have been commercially applied include rutile crystal, lithium niobate crystal, yttrium vanadate crystal, calcite crystal, silicon dioxide crystal, magnesium fluoride crystal and α-BaB2O4 crystal. Yttrium vanadate crystal is a crystal with excellent performance, but its ultraviolet cutoff edge is above 400nm, and its transmittance to the bands below 400nm is very poor, so it cannot be used in the ultraviolet and deep ultraviolet bands. Magnesium fluoride crystal has a long transmittance range (110nm~8500nm) and is the only birefringent crystal that can be used in the ultraviolet and deep ultraviolet bands, but its birefringence is small, which seriously affects its application. Silicon dioxide crystals are also troubled by the size of the birefringence. The α-BaB2O4 crystal has a wide spectral transmittance range (189nm~3500nm), contains a short ultraviolet cutoff edge, and a large birefringence (0.159@253.7nm). It has important application value in the ultraviolet region. However, the crystal undergoes phase change at high temperature, is very easy to crack during the growth process, and it is not easy to obtain large-sized single crystals.

[0004] With the development of science and technology, people have higher and higher requirements for birefringent crystals. It is very important to find an excellent birefringent crystal in terms of both quality and quantity. Excellent birefringent crystals require that they are easy to process and grow, have a large birefringence and transmittance, and have stable physical and chemical properties. Therefore, scientific researchers have been constantly exploring and trying in recent years, and are committed to finding an excellent birefringent crystal material and using it in practical applications. Summary of the invention

[0005] According to one aspect of the present application, a crystal material is provided, and the first principle calculation shows that the crystal has a large birefringence. The birefringence at 1042nm is 0.241. The birefringent crystal material 4(C3N6H6)·HPF6·4H2O provided by the present invention has good transmittance in a wide spectrum range of 200nm to 2500nm.

[0006] A crystalline material, wherein the chemical formula of the crystalline material is 4(C3N6H6)·HPF6·4H2O;

[0007] C3N6H6 are connected by intramolecular NH···N hydrogen bonds;

[0008] PF6 - It is connected with C3N6H6 through intramolecular hydrogen bonds to form a three-dimensional structure.

[0009] Optionally, the crystalline material is a single crystal structure.

[0010] Optionally, the crystalline material belongs to the triclinic system, and the space group is

[0011] Optionally, the unit cell parameters of the crystal material are as follows:

[0012] α=69.387(6)°, β=89.230(6)°, γ=73.113(6)°.

[0013] Optionally, the crystalline material has a birefringence of 0.230 to 0.245 at 1042 nm according to first principle calculations.

[0014] According to a second aspect of the present application, a method for preparing a crystalline material is provided.

[0015] The method for preparing the above-mentioned crystal material comprises the following steps:

[0016] A mixture containing melamine, a hexafluorophosphate compound and water is reacted to obtain the crystalline material by adjusting the pH value of the solution to a weak acidity;

[0017] The molar ratio of the melamine to the hexafluorophosphate compound is 4:1 to 4.5:1;

[0018] The molar volume ratio of melamine to water is 1mmol:40mL to 1:60mL.

[0019] Optionally, the molar ratio of the melamine to the hexafluorophosphate compound is independently selected from any value of 4:1, 4:2, 4:3, 4:4, 4:5, or any range between two of them.

[0020] Optionally, the molar volume ratio of melamine to water is independently selected from any value among 1mmol:40mL, 1mmol:42mL, 1mmol:45mL, 1mmol:50mL, 1mmol:52mL, 1mmol:55mL, 1mmol:60mL, or any range value therebetween.

[0021] Optionally, the hexafluorophosphate compound is selected from at least one of LiPF6, NaPF6, KPF6, CsPF6, and HPF6.

[0022] Optionally, the reaction conditions are as follows:

[0023] Temperature is 40℃~90℃;

[0024] The time is 40min to 50min.

[0025] Optionally, the reaction temperature is independently selected from any value of 40°C, 42°C, 50°C, 55°C, 60°C, 65°C, 70°C, 80°C, 90°C, or any range therebetween.

[0026] Optionally, the reaction time is independently selected from any value of 40 min, 42 min, 43 min, 44 min, 45 min, 46 min, 47 min, 48 min, 49 min, 50 min, or any range therebetween.

[0027] According to a third aspect of the present application, an application of a crystalline material is provided.

[0028] Application of the above-mentioned crystal material and / or the crystal material obtained by the above-mentioned preparation method in the preparation of polarization beam splitting prisms or optical elements.

[0029] Optionally, the polarization beam splitter prism is selected from one of a Glan-type prism, a Wollaston prism, a Rochon prism, and a beam splitting polarizer;

[0030] The optical element is selected from one of an optical isolator, a circulator, a beam displacer, an optical polarizer, an optical modulator, an optical polarizer, a polarization beam splitter, a phase delay device, and an electro-optical modulation device.

[0031] The beneficial effects of this application include:

[0032] 1) A crystal material provided in the present application has a large birefringence index as shown by first principle calculation. The birefringence index at 1042nm is 0.241; the birefringent crystal material 4(C3N6H6)·HPF6·4H2O provided by the present invention has good transmittance in a wide spectrum range of 200nm to 2500nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the structure of the 4(C3N6H6)·HPF6·4H2O crystal obtained in Examples 1-3.

[0034] Figure 2This is the birefringence spectrum of the 4(C3N6H6)·HPF6·4H2O crystal obtained in Example 1-3.

[0035] Figure 3 This is a schematic diagram of the polarization beam splitter prism made in Example 4. DETAILED DESCRIPTION

[0036] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0037] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0038] The analysis method in the examples of this application is as follows:

[0039] The crystal structure data was tested using a Rigaku ROD, Synergy Custom system four-circle diffractometer with a wavelength of Ga Kα rays. Data collection was performed at room temperature;

[0040] The birefringence data of the crystal were obtained by first-principle calculations using Materials Studio 8.0 software, with all parameters set to default values ​​without further adjustment.

[0041] Example 1

[0042] A method for preparing 4(C3N6H6)·HPF6·4H2O birefringent crystal by aqueous solution method comprises the following steps:

[0043] 1) Dissolve 4.5 mmol of melamine and 1 mmol of sodium hexafluorophosphate in a clean beaker containing 60 mL of water, and adjust the pH value of the solution to weak acidity;

[0044] 2) The mixed aqueous solution was placed on a magnetic stirrer and heated to 60 degrees Celsius, and stirred continuously for 40 minutes during the heating process. Then it was placed at room temperature to cool and crystallize. After three to five days, a large number of colorless transparent single crystals appeared.

[0045] 3) The crystals obtained in step 2) were washed with pure water and then dried naturally. The sample obtained in Example 1 was placed on a four-circle diffractometer to collect diffraction data. The crystal structure obtained after software restoration and data refinement was as follows: Figure 1 shown.

[0046] 4) The single crystal data obtained in step 3) was calculated by first principle, and the first principle calculation showed that the compound had a large birefringence, and the birefringence at 1042 nm was 0.241.

[0047] Example 2

[0048] A method for preparing 4(C3N6H6)·HPF6·4H2O birefringent crystal by aqueous solution method comprises the following steps:

[0049] 1) Dissolve 4.2 mmol of melamine and 1 mmol of potassium hexafluorophosphate in a clean beaker containing 50 mL of water, and adjust the pH value of the solution to weak acidity;

[0050] 2) The mixed aqueous solution was placed on a magnetic stirrer and heated to 50 degrees Celsius, and stirred continuously for 45 minutes during the heating process. Then it was placed at room temperature to cool and crystallize. After three to five days, a large number of colorless transparent single crystals appeared.

[0051] 3) The crystals obtained in step 2) were washed with pure water and then dried naturally. The sample obtained in Example 2 was placed on a four-circle diffractometer to collect diffraction data. The crystal structure obtained after software restoration and data refinement was as follows: Figure 1 shown.

[0052] 4) The single crystal data obtained in step 3) was calculated by first principle, and the first principle calculation showed that the compound had a large birefringence, and the birefringence at 1042 nm was 0.241.

[0053] Example 3

[0054] A method for preparing 4(C3N6H6)·HPF6·4H2O birefringent crystal by aqueous solution method comprises the following steps:

[0055] 1) Dissolve 4 mmol of melamine and 1 mmol of lithium hexafluorophosphate in a clean beaker containing 40 mL of water, and adjust the pH value of the solution to weak acidity;

[0056] 2) The mixed aqueous solution is placed on a magnetic stirrer and heated to 80 degrees Celsius, and stirred continuously for 40 minutes during the heating process. Then it is placed at room temperature to cool and crystallize. After three to five days, a large number of colorless transparent single crystals appear.

[0057] 3) The crystals obtained in step 2) were washed with pure water and then dried naturally. The sample obtained in Example 3 was placed on a four-circle diffractometer to collect diffraction data. The crystal structure obtained after software restoration and data refinement was as follows: Figure 1 shown.

[0058] 4) The single crystal data obtained in step 3) was calculated by first principle, and the first principle calculation showed that the compound had a large birefringence, and the birefringence at 1042 nm was 0.241.

[0059] Example 4 Polarizing Prism

[0060] Any 4(C3N6H6)·HPF6·4H2O crystals obtained in Examples 1-3 are processed and bonded together to make a Figure 3 Polarizing prism. When the light beam is incident vertically on the prism surface, neither the o-light nor the e-light is deflected in prism 1; the o-light is completely reflected at the glued surface and is completely absorbed by the absorption coating on the prism surface, while the e-light is emitted from the second prism.

[0061] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A crystalline material, characterized in that: The chemical formula of the crystalline material is 4(C3N6H6)·HPF6·4H2O; C3N6H6 are connected by intramolecular NH···N hydrogen bonds; (PF6) - It forms a three-dimensional structure by connecting with C3N6H6 through intramolecular hydrogen bonds; The crystal material belongs to the triclinic system, and the space group is The unit cell parameters of the crystal material are as follows: α=69.387(6)°, β=89.230(6)°, γ=73.113(6)°.

2. The crystalline material according to claim 1, characterized in that The crystal material is a single crystal structure.

3. The crystal material according to claim 1, characterized in that The crystal material has a birefringence of 0.230 to 0.245 at 1042 nm according to first principle calculations.

4. The method for preparing a crystalline material according to any one of claims 1 to 3, characterized in that: The following steps are involved: Mixing raw materials containing melamine, a hexafluorophosphate compound, and water to obtain a solution, adjusting the pH value of the solution to weak acidity, and obtaining the crystalline material after reaction; The molar ratio of the melamine to the hexafluorophosphate compound is 4:1 to 4.5:1; The reaction conditions are as follows: Temperature is 40℃~90℃; The time is 40min to 50min.

5. The preparation method according to claim 4, characterized in that: The hexafluorophosphate compound is selected from at least one of LiPF6, NaPF6, KPF6, CsPF6, and HPF6.

6. Use of the crystal material according to any one of claims 1 to 3 and / or the crystal material obtained by the preparation method according to any one of claims 4 to 5 in the preparation of a polarization beam splitter prism.

7. The use according to claim 6, characterized in that: The polarization beam splitter prism is selected from one of a Glan prism, a Wollaston prism, a Rochon prism, and a beam splitting polarizer.

8. Use of the crystal material according to any one of claims 1 to 3 and / or the crystal material obtained by the preparation method according to any one of claims 4 to 5 in the preparation of optical elements.

9. The use according to claim 8, characterized in that: The optical element is selected from one of an optical isolator, a circulator, a beam displacer, an optical polarizer, an optical modulator, an optical polarizer, a polarization beam splitter, a phase delay device, and an electro-optical modulation device.