A catalytic cracking aid containing large particle size sol and preparation method thereof
By using large particle size sol in the catalytic cracking aid to form a rich mesoporous structure, the problem of low selectivity of carbon tetraolefins in the existing technology is solved, the yield and selectivity of carbon tetraolefins are significantly improved, and the Catalyst wear resistance.
Patent Information
- Application Number
- CN202111208517.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-18
AI Technical Summary
Existing catalytic cracking catalysts for increasing the production of low-carbon olefins rely on increasing the yield of liquefied gas to increase the yield of carbon tetraolefins. However, the selectivity of carbon tetraolefins is low and the lack of rich meso-macropore structure makes it difficult for carbon tetraolefins to diffuse quickly, resulting in the production of carbon tetraolefins. Rate and selectivity decrease.
Provided is a catalytic cracking aid containing large particle size sol, containing 15 to 50% by weight of beta zeolite, 10 to 75% by weight of clay, and 10 to 50% by weight of large particle size sol, with an average particle size distribution of 20 to 20% by weight. Large particle size sol in the range of 50nm accounts for more than 60% of the total amount, forming a rich mesoporous structure and improving the yield and selectivity of carbon tetraolefins.
Through the rich mesoporous structure, low-carbon olefins such as carbon tetraolefins can quickly diffuse, avoid secondary reactions, significantly increase the yield and selectivity of carbon tetraolefins, and improve the wear resistance and bonding properties of the catalyst.
Smart Images

Figure CN115990496B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of oil refining industry, and in particular relates to a catalytic cracking aid containing a large-particle sol and a preparation method thereof. Background Art
[0002] The transformation of oil refining to basic chemical raw materials such as olefins and aromatics has become the mainstream of the industry. Catalytic cracking is one of the key technologies for maximizing the production of low-carbon olefins from crude oil. According to statistics, nearly 70% of the world's C4 olefins come from catalytic cracking units, and the technology for producing C4 olefin fractions from catalytic cracking units has the advantages of low investment and low cost. Many companies are trying to obtain a larger amount of C4 olefin yield from the catalytic cracking process. Catalytic cracking catalysts or additives are the most direct and economical way to increase the yield of C4 olefins.
[0003] The main active components of the catalytic cracking catalyst or additive for increasing the production of C4 olefins are Y-type molecular sieve, ZSM-5 molecular sieve and β-zeolite. Among them, β-zeolite is used as the main active component of the catalyst for increasing the production of C4 olefins due to its special structure, which has both acid catalytic properties and structural selectivity. Binder is also one of the main components of the catalytic cracking catalyst or additive. While ensuring the wear resistance of the catalyst, it can synergize with the active components to improve the activity and hydrothermal stability of the catalyst. The most commonly used binders are aluminum sol, silica sol, acidified pseudo-boehmite, etc.
[0004] US6355591 discloses a catalytic cracking aid containing 4-20 wt% aluminum phosphate, 1-40 wt% ZSM-5, Beta zeolite and a mixture thereof, and 40-90 wt% clay, which can increase the yield of liquefied gas.
[0005] CN1055105C discloses a cracking catalyst for producing more isobutylene and isopentene, which contains 6-30% by weight of five-membered ring high-silicon zeolite containing phosphorus and rare earth, 5-20% by weight of USY zeolite, 1-5% by weight of beta zeolite, 30-60% by weight of clay and 15-30% by weight of inorganic oxides. The catalyst has the characteristics of producing more isobutylene and isopentene under the process conditions of catalytic cracking, and can also co-produce high-octane gasoline.
[0006] CN103785456A discloses a cracking aid for increasing the concentration of light olefins, comprising a modified beta molecular sieve, a phosphorus-aluminum inorganic binder containing a first clay, other inorganic binders and a Group VIII metal additive, with or without a second clay; the phosphorus-aluminum inorganic binder containing the first clay comprises an aluminum component, a phosphorus component and a first clay; the phosphorus-and-transition metal modified beta molecular sieve has a phosphorus content of 1 to 10% by weight in terms of P2O5 and a metal content of 0.5 to 10% by weight in terms of metal oxide. The cracking catalyst composition is applied to the catalytic cracking of petroleum hydrocarbons, can increase the yield of catalytic cracking liquefied gas, increase the concentration of light olefins in liquefied gas, especially the concentration of isobutylene, and at the same time increase the ratio of ethylene to dry gas, increase the octane number of gasoline, and do not affect the heavy oil conversion capacity of the main catalyst when the additive is mixed in a large proportion.
[0007] Although the existing catalytic cracking catalysts or additives for increasing the production of low-carbon olefins can achieve the purpose of increasing the production of C4 olefins to a certain extent, the following problems still exist: the C4 olefin yield is mainly increased by increasing the liquefied gas yield, while the C4 olefin concentration in the liquefied gas does not change much and the C4 olefin selectivity is low; the catalysts or additives lack rich medium and large pore structures, which is not conducive to the rapid diffusion of C4 olefins generated in the catalytic cracking process, resulting in the continued secondary reaction of low-carbon olefins such as C4 olefins, resulting in a decrease in their yield and selectivity.
[0008] Therefore, in order to solve the above problems, the purpose of the present invention is to provide a catalytic cracking aid with rich mesoporous structure and a preparation method thereof, so as to further improve the yield and selectivity of C4 olefins. Summary of the invention
[0009] In one aspect, the present invention provides a catalytic cracking aid comprising a large-particle sol, wherein the catalytic cracking aid comprises, based on the dry weight of the catalytic cracking aid, 15 to 50 weight percent of beta zeolite, 10 to 75 weight percent of clay, and 10 to 50 weight percent of the large-particle sol, wherein the large-particle sol (on a dry basis) comprises 10 to 40 weight percent of Al2O3, 50 to 85 weight percent of P2O5, and 0.2 to 10 weight percent of SiO2, wherein P2O5 is 0.1 to 0.2 ... The mass ratio of SiO2:Al2O3 is (1.5-5.0):1, the mass ratio of SiO2:Al2O3 is (0.01-0.3):1, the large-particle sol with an average particle size distribution in the range of 20-50 nm accounts for more than 60% of the total number, and the pore distribution is determined by a low-temperature nitrogen adsorption method. The total pore volume of the catalytic cracking aid is not less than 0.200 mL / g, wherein the pore volume of mesopores with a pore size of 4-50 nm accounts for more than 60% of the total pore volume.
[0010] In one embodiment, the catalytic cracking aid according to the present invention contains 20-40 wt% of beta zeolite, 20-65 wt% of clay and 15-45 wt% of large particle size sol.
[0011] In one embodiment, according to the catalytic cracking aid of the present invention, the large-particle sol contains 15-35 weight % of Al2O3, 55-80 weight % of P2O5 and 0.5-8.0 weight % of SiO2, wherein the mass ratio of P2O5:Al2O is (2.0-4.5):1, the mass ratio of SiO2:Al2O3 is (0.05-0.25):1, and the large-particle sol with an average particle size distribution in the range of 25-45 nm accounts for more than 60% of the total number.
[0012] In one embodiment, according to the catalytic cracking aid of the present invention, the total pore volume of the catalytic cracking aid is 0.200-0.300 mL / g.
[0013] In one embodiment, according to the catalytic cracking aid of the present invention, the pore volume of mesopores with a size of 4 to 50 nm accounts for 65 to 85% of the total pore volume.
[0014] In one embodiment, according to the catalytic cracking aid of the present invention, the β zeolite is selected from hydrogen β zeolite, sodium β zeolite, phosphorus-modified β zeolite, metal-modified β zeolite or any combination thereof, and the molar ratio of SiO2 to Al2O3 in the β zeolite is 20-50.
[0015] In one embodiment, according to the catalytic cracking aid of the present invention, the beta zeolite is hydrogen beta zeolite.
[0016] In one embodiment, according to the catalytic cracking aid of the present invention, the metal in the metal-modified beta zeolite is selected from La, Ce, Pr, Zr, Ti, Fe, Cu, and Mg.
[0017] In one embodiment, according to the catalytic cracking aid of the present invention, the clay is selected from kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite, sepiolite or any combination thereof.
[0018] On the other hand, the present invention provides a method for preparing the aforementioned catalytic cracking aid, comprising the following steps:
[0019] (1) First, prepare a large particle size sol, the steps are as follows:
[0020] (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25 weight percent;
[0021] (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the second slurry has a solid content of 15 to 50% by weight;
[0022] (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight;
[0023] (1d) placing the third slurry at 20 to 60° C. for 1 to 72 hours for aging to obtain the large-particle sol;
[0024] The mass ratio of the phosphorus source calculated as P2O5 to the aluminum source is (1.5-5.0):1, and the mass ratio of the silica sol calculated as SiO2 to the aluminum source calculated as Al2O3 is (0.01-0.3):1;
[0025] (2) Then, the clay, β zeolite and the large-particle sol are fully mixed to obtain a slurry, wherein the solid content of the obtained slurry is 10 to 50% by weight, and the slurry is spray-dried, formed and calcined to obtain the aforementioned catalytic cracking aid, wherein, on a dry basis, the weight ratio of the β zeolite, the clay and the large-particle sol is (15 to 50):(10 to 75):(10 to 50).
[0026] In one embodiment, according to the preparation method of the present invention, in step (1a), the mixing and stirring is performed for 30 to 60 minutes.
[0027] In one embodiment, according to the preparation method of the present invention, step (1b) is carried out at a temperature of 35 to 55° C., and the mixing and stirring is carried out for 30 to 90 minutes.
[0028] In one embodiment, according to the preparation method of the present invention, step (1c) is carried out at a temperature of 35 to 55° C., and the mixing and stirring is carried out for 30 to 90 minutes.
[0029] In one embodiment, according to the preparation method of the present invention, the aluminum source is selected from one or more of pseudo-boehmite, alumina, boehmite, gibbsite and diaspore.
[0030] In one embodiment, according to the preparation method of the present invention, the phosphorus source is selected from one or more of phosphoric acid, phosphorous acid and hypophosphorous acid.
[0031] In one embodiment, according to the preparation method of the present invention, the clay is selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.
[0032] In one embodiment, according to the preparation method of the present invention, the β zeolite is selected from hydrogen β zeolite, sodium β zeolite, phosphorus-modified β zeolite, metal-modified β zeolite or any combination thereof, and the molar ratio of SiO2 to Al2O3 in the β zeolite is 20-50.
[0033] In another aspect, the present invention provides a large-particle sol, which contains, based on its dry weight, 10-40 wt% of Al2O3, 50-85 wt% of P2O5 and 0.2-10 wt% of SiO2, wherein the mass ratio of P2O5:Al2O3 is (1.5-5.0):1, the mass ratio of SiO2:Al2O3 is (0.01-0.3):1, and the average particle size is 20-50 nm, and is prepared as follows:
[0034] (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25 weight percent;
[0035] (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the second slurry has a solid content of 15 to 50% by weight;
[0036] (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight; and
[0037] (1d) placing the third slurry at 20-60° C. for 1-72 hours for aging treatment to obtain the large-particle sol.
[0038] The catalytic cracking aid prepared according to the method of the present invention, as mentioned above, comprises a large-particle sol, which is formed by piling up colloid particles with large and uniform particle sizes to form a rich mesoporous structure. Therefore, the catalytic cracking aid comprising the large-particle sol of the present invention is used in a catalytic cracking process, and low-carbon olefins such as C4 olefins can be rapidly diffused out through the rich mesoporous structure of the aid, thereby avoiding its continued secondary reaction, thereby achieving an increase in the yield and selectivity of low-carbon olefins such as C4 olefins. In addition, the large-particle sol included in the catalytic cracking aid of the present invention is distributed on molecular sieves and clay, which can further improve the bonding performance and improve the wear resistance, i.e., strength, of the aid. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a TEM picture of the catalytic cracking aid A1 prepared according to Example 1.
[0040] Figure 2 This is a TEM photo of the catalytic cracking aid DA3 prepared according to Comparative Example 3.
[0041] Figure 3 The pore size distribution diagram of the catalytic cracking aid prepared according to Example 3 and Comparative Example 3. DETAILED DESCRIPTION
[0042] The present invention will be further described in detail below through the accompanying drawings and embodiments. Through these descriptions, the characteristics and advantages of the present invention will become more clear and distinct.
[0043] In addition, the technical features involved in different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0044] On the one hand, the present invention provides a catalytic cracking aid comprising a large-particle sol. Based on the dry weight of the catalytic cracking aid, the catalytic cracking aid contains 15 to 50 weight percent of beta zeolite, 10 to 75 weight percent of clay, and 10 to 50 weight percent of large-particle sol. The large-particle sol contains 10 to 40 weight percent of Al2O3, 50 to 85 weight percent of P2O5, and 0.2 to 10 weight percent of SiO2, wherein the mass ratio of P2O5:Al2O is (1.5 to 5.0):1, and the mass ratio of SiO2:Al2O3 is (0.01 to 0.3):1. The large-particle sol with an average particle size distribution in the range of 20 to 50 nm accounts for more than 60% of the total number. The pore distribution is determined by a low-temperature nitrogen adsorption method. The total pore volume of the catalytic cracking aid is not less than 0.200 mL / g, wherein the pore volume of pores in the range of 4 to 50 nm accounts for more than 60% of the total pore volume.
[0045] The catalytic cracking aid according to the present invention preferably contains 20-40 wt% of beta zeolite, 20-65 wt% of clay and 15-45 wt% of large-particle sol. The large-particle sol preferably contains 15-35 wt% of Al2O3, 55-80 wt% of P2O5 and 0.5-8.0 wt% of SiO2, wherein the mass ratio of P2O5:Al2O is preferably (2.0-4.5):1, and the mass ratio of SiO2:Al2O3 is preferably (0.05-0.25):1. The large-particle sol with an average particle size distribution in the range of 25-45 nm can account for more than 60% of the total number. The total pore volume of the catalytic cracking aid according to the present invention can reach 0.200-0.300 mL / g, wherein the pore volume of 4-50 nm mesopores can account for 65-85% of the total pore volume.
[0046] The beta zeolite contained in the catalytic cracking aid of the present invention is selected from hydrogen beta zeolite, sodium beta zeolite, phosphorus-modified beta zeolite, metal-modified beta zeolite or any combination thereof, preferably hydrogen beta zeolite. The metal in the metal-modified beta zeolite contained in the catalytic cracking aid of the present invention may be, for example, a rare earth metal, etc., for example, selected from La, Ce, Pr, Zr, Ti, Fe, Cu, Mg. The clay contained in the catalytic cracking aid of the present invention may be various clays suitable for catalyst preparation well known to those skilled in the art, for example, selected from kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite, sepiolite or any combination thereof.
[0047] On the other hand, the present invention provides a method for preparing the aforementioned catalytic cracking aid, comprising the following steps:
[0048] (1) First, prepare a large particle size sol, the steps are as follows:
[0049] (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25 weight percent;
[0050] (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the second slurry has a solid content of 15 to 50% by weight;
[0051] (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight;
[0052] (1d) placing the third slurry at 20 to 60° C. for 1 to 72 hours for aging to obtain the large-particle sol;
[0053] The mass ratio of the phosphorus source calculated as P2O5 to the aluminum source is (1.5-5.0):1, and the mass ratio of the silica sol calculated as SiO2 to the aluminum source calculated as Al2O3 is (0.01-0.3):1;
[0054] (2) Then, the clay, β zeolite and the large-particle sol are fully mixed to obtain a slurry, wherein the solid content of the obtained slurry is 10 to 50% by weight, and the slurry is spray-dried, formed and calcined to obtain the aforementioned catalytic cracking aid, wherein, on a dry basis, the weight ratio of the β zeolite, the clay and the large-particle sol is (15 to 50):(10 to 75):(10 to 50).
[0055] In the preparation method of the present invention, the aluminum source used in step (1a) is selected from one or more of pseudo-boehmite, alumina, aluminum nitrate, aluminum isopropoxide, boehmite, gibbsite and diaspore; the mixing and stirring time of the aluminum source and deionized water is preferably in the range of 30 to 60 minutes.
[0056] In the preparation method of the present invention, the phosphorus source used in step (1b) is selected from one or more of phosphoric acid, phosphorous acid and hypophosphorous acid; the first slurry prepared in step (1a) is preferably mixed and stirred with the phosphorus source at a temperature of 35 to 55° C., and the mixing and stirring time is preferably 30 to 90 minutes.
[0057] In the preparation method of the present invention, it is preferred that the selected aluminum source can interact with the selected phosphorus source to form aluminum phosphates of different forms.
[0058] In the preparation method of the present invention, step (1c) is preferably carried out at a temperature of 35 to 55° C., and the mixing and stirring time of the second slurry prepared in step (1b) and the silica sol is preferably 30 to 90 minutes.
[0059] In the preparation method of the present invention, OH on the surface of the aluminum source absorbs H+ in phosphoric acid to form positively charged colloid particles, which repel each other and break up and dismember, and under the action of surface tension, a large number of colloid particles with an average particle size of 20 to 50 nm are formed; adding silica sol particles is beneficial to inhibiting further aggregation of the colloid particles and improving the stability of the colloidal structure.
[0060] In the preparation method of the present invention, the selection of clay and beta zeolite used in step (2) is the same as described above for the catalytic cracking aid of the present invention.
[0061] In the preparation method of the present invention, the molding and drying performed in step (2) refers to the granulation molding and drying of the catalyst, which is a technology well known to those skilled in the art. The preparation of catalytic cracking catalyst generally uses spray molding and drying, and the temperature of the spray tail gas is controlled at 100-250°C. The calcination treatment is also well known to those skilled in the art. For example, it can be carried out in a muffle furnace, and the following calcination treatment conditions are adopted: the temperature is 350-800°C, preferably 400-650°C, and the calcination time is 0.5-6 hours, preferably 1-4 hours. The calcination can be carried out in any atmosphere, for example, in air or inert atmosphere. The inert atmosphere contains inert gas, and the inert gas may include nitrogen, helium, argon, etc.
[0062] When the catalytic cracking aid according to the present invention is used in a catalytic cracking process, it can be added to the catalytic cracking reactor alone or mixed with the catalytic cracking catalyst. When mixed with the catalytic cracking catalyst, the amount of the catalytic cracking aid is preferably 1 to 50% by weight, more preferably 5 to 40% by weight, based on the total amount of the catalytic cracking aid and the catalytic cracking catalyst.
[0063] In general, compared with the prior art, the catalytic cracking aid according to the present invention has a rich mesoporous structure, and the pore volume of 4-50 nm mesopores accounts for more than 60% of the total pore volume. It is used in the catalytic cracking process, which is beneficial to improve the diffusion capacity of raw material molecules and product molecules, thereby significantly improving the yield and selectivity of C4 olefins.
[0064] Specifically, the rich mesoporous structure of the catalytic cracking aid according to the present invention mainly comes from the pore structure generated by the accumulation of colloidal particles of the large-particle sol contained in its composition. The large-particle sol contained in the catalytic cracking aid according to the present invention has at least two functions: on the one hand, it is distributed on the surface of the β-zeolite molecular sieve and the clay, giving full play to the bonding performance and enhancing the strength of the catalyst aid; on the other hand, the colloidal particles are accumulated to form a pore structure. Since the colloidal particle size of the large-particle sol contained in the present invention is concentrated in the range of 20 to 50 nm, the accumulation of the large-particle particles can form a rich mesoporous structure, while the particle size of conventional sols such as aluminum sol and acidified pseudo-boehmite is generally less than 5 nm, and the accumulation of smaller-particle particles cannot form a rich mesoporous structure, and even blocks the pore structure of the molecular sieve.
[0065] Furthermore, by Figures 1 to 3 It can be seen from the TEM photos and the average particle size distribution diagram that the conventional aluminum phosphate sol prepared according to the prior art has an uneven particle size distribution and a small particle size, usually less than 10 nm. In comparison, the large-particle sol prepared in the preparation method of the present invention has a larger particle size (20 to 50 nm) and is evenly distributed, thereby overcoming the problem that the existing aluminum phosphate sol has a small particle size and uneven distribution, resulting in an unclear pore structure in the catalyst.
[0066] The present invention is further described below by way of examples, which are intended to help those skilled in the art better understand the essence of the present invention and the beneficial effects brought about by it, but should not be construed as constituting any limitation on the practicable scope of the present invention.
[0067] Example
[0068] The raw materials used in the following examples and comparative examples are described as follows:
[0069] Kaolin was produced by Suzhou Kaolin Company with a solid content of 76% by weight;
[0070] Pseudo-boehmite was produced by Shandong Aluminum Plant and had a solid content of 62% by weight;
[0071] The solid content of the silica sol is 27% by weight, and the pH is 2 to 3;
[0072] The solid content of hydrogen-type beta zeolite is 75% by weight, the SiO2 / Al2O3 molar ratio is 25, and the Na2O content is 0.15% by weight;
[0073] Phosphoric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 85%.
[0074] Specific surface area and pore volume analysis: The ASAP 2405N V1.01 automatic adsorption instrument from Micromeritics, USA, was used, and the low temperature static nitrogen adsorption capacity method was used. The sample was heated to 1.33×10 -2 Pa, vacuum degassing at 300℃ for 4h, using N2 as adsorption medium, and measuring the adsorption-desorption isotherm of the sample at 77.4K. Calculate the specific surface area of the sample according to the BET formula, measure the volume of N2 adsorbed by the sample when the relative pressure p / p0=0.98, convert it into liquid nitrogen volume, that is, the total pore volume, and calculate the micropore volume according to the t-plot method. The difference between the two is the volume of 2-100nm macropores, among which the pore volume of 4-50nm mesopores is obtained by the peak fitting method. The pore size distribution is calculated using the BJH desorption pore size distribution data.
[0075] Measurement of colloid particle size: The JEM-2000FX-II transmission electron microscope of Japan Electronics Company was used for analysis. The average particle size of the colloid particles was obtained by randomly measuring 10 projections of the colloid particles in the TEM image of the sample and taking the average value of the maximum circumscribed circle diameter.
[0076] Additive strength: put a certain amount of additive into a fixed device and blow it for 5 hours under a constant airflow. Except for the first hour, the average wear percentage in the last four hours is called the additive wear index, and the unit is % per hour. The method and standard are: air lift method Q / SYLS0518-2002.
[0077] Evaluation of catalytic cracking aid: The catalytic cracking aid was pre-aged in a fixed bed aging device at 800°C and 100% by volume steam for 17 hours, and then evaluated on the ACE device. The properties of the reaction raw oil are shown in Table 4. The reaction temperature is 500°C, the agent-oil weight ratio is 6, and the mass space velocity is 16s -1 Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield, C4 olefin selectivity = C4 olefin yield / conversion rate.
[0078] The following Examples 1 to 5 are examples of preparing large particle sols according to the method of the present invention.
[0079] Example 1
[0080] First, 493 g of pseudo-boehmite and 1546 g of deionized water were mixed at room temperature (25°C) and stirred for 60 min to obtain a first slurry with a solid content of 15 wt%; then, 727 g of 85 wt% phosphoric acid solution was added to the first slurry, and the mixture was stirred at 45°C for 60 min to obtain a second slurry with a solid content of 33 wt%; then, 283 g of silica sol was added to the second slurry, and the mixture was stirred at 45°C for 45 min to obtain a third slurry with a solid content of 33 wt%; finally, the third slurry was placed at 45°C and allowed to stand for 48 h to obtain a large-particle sol A1 according to the method of the present invention.
[0081] Example 2
[0082] First, 413 g of pseudo-boehmite and 868 g of deionized water were mixed at room temperature and stirred for 90 min, to obtain a first slurry with a solid content of 15 wt %; then, 839 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 50° C. for 60 min, to obtain a second slurry with a solid content of 38 wt %; then, 114 g of silica sol was added to the second slurry, and the mixture was stirred at 50° C. for 30 min, to obtain a third slurry with a solid content of 38 wt %; finally, the third slurry was placed at 50° C. and allowed to stand for 12 h, to obtain a large-particle sol A2 according to the method of the present invention.
[0083] Example 3
[0084] First, 363 g of pseudo-boehmite and 1888 g of deionized water were mixed at room temperature and stirred for 60 min, to obtain a first slurry with a solid content of 10 wt %; then, 885 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 55° C. for 60 min, to obtain a second slurry with a solid content of 31 wt %; then, 83 g of silica sol was added to the second slurry, and the mixture was stirred continuously at 55° C. for 60 min, to obtain a third slurry with a solid content of 31 wt %; the third slurry was placed at 40° C. and allowed to stand for 24 h, to obtain a large-particle sol A3 according to the method of the present invention.
[0085] Example 4
[0086] First, 299 g of pseudo-boehmite and 2017 g of deionized water were mixed at room temperature and stirred for 45 min, to obtain a first slurry with a solid content of 8 wt %; then, 911 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 50° C. for 90 min, to obtain a second slurry with a solid content of 30 wt %; then, 151 g of silica sol was added to the second slurry, and the mixture was stirred at 50° C. for 30 min, to obtain a third slurry with a solid content of 30 wt %; the third slurry was placed at 35° C. and allowed to stand for 24 h, to obtain a large-particle sol A4 according to the method of the present invention.
[0087] Example 5
[0088] First, 268 g of pseudo-boehmite and 3059 g of deionized water were mixed at room temperature and stirred for 60 min, to obtain a first slurry with a solid content of 5 wt %; then, 979 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 60° C. for 90 min, to obtain a second slurry with a solid content of 23 wt %; then, 6 g of silica sol was added to the second slurry, and the mixture was stirred at 60° C. for 30 min, to obtain a third slurry with a solid content of 23 wt %; the third slurry was placed at 60° C. and allowed to stand for 12 h, to obtain a large-particle sol A5 according to the method of the present invention.
[0089] Comparative Example 1
[0090] A comparative sol was prepared according to the method of Example 1, except that no silica sol was added.
[0091] First, 534 g of pseudo-boehmite and 1674 g of deionized water were mixed at room temperature and stirred for 60 min to obtain a first slurry with a solid content of 15 wt %; then, 787 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 45°C for 60 min to obtain a second slurry with a solid content of 33 wt %; the second slurry was placed at 45°C and allowed to stand for 48 h to obtain a comparison sol DA1.
[0092] Comparative Example 2
[0093] A comparative sol was prepared according to the method of Example 1, except that no aging treatment was performed.
[0094] First, 493 g of pseudo-boehmite and 1546 g of deionized water were mixed at room temperature and stirred for 60 min, to obtain a first slurry with a solid content of 15 wt %; then, 727 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 45°C for 60 min, to obtain a second slurry with a solid content of 33 wt %; then, 283 g of silica sol was added to the second slurry, and the mixture was stirred at 45°C for 45 min, to obtain a third slurry with a solid content of 33 wt %, namely, comparison sol DA2.
[0095] Comparative Example 3
[0096] A comparative sol was prepared according to the method of Example 1 in CN1417296A, which differed from the above Examples 1 to 5 in that no silica sol was added and no aging treatment was performed.
[0097] 534 g of pseudo-boehmite and 1674 g of deionized water were mixed at room temperature and stirred for 30 min. 787 g of 85 wt% phosphoric acid solution was added to the slurry while stirring. The mixture was stirred at 70° C. for 45 min to obtain a colorless and transparent phosphorus-containing aluminum sol, namely, comparison sol DA3.
[0098] The physicochemical properties of the sols obtained in Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 1. The TEM photos of the sols obtained in Example 1 and Comparative Example 3 are shown in Figure 1 and Figure 2 .
[0099] Table 1 Composition and properties of the sols obtained in Examples 1 to 5 and Comparative Examples 1 to 3
[0100] Sol Name A1 A2 A3 A4 A5 DA1 DA2 DA3 <![CDATA[P2O5, wt%]]> 61.8 71.3 75.2 77.4 83.2 66.9 61.8 66.9 <![CDATA[Al2O3, wt%]]> 30.6 25.6 22.5 18.5 16.6 33.1 30.6 33.1 <![CDATA[SiO2, wt%]]> 7.6 3.1 2.3 4.1 0.2 0.0 7.6 0.0 Average particle size, nm 35 40 38 30 25 12 15 5
[0101] From Table 1 and Figure 1 and 2 It can be seen that compared with the comparative example, the sol particle size obtained according to the preparation method of the present invention is larger and more evenly distributed, which is helpful to form a mesoporous structure and improve the yield and selectivity of C4 olefins.
[0102] The following Examples 6 to 10 are preparation examples of the catalytic cracking aid containing large particle size sol of the present invention.
[0103] Example 6
[0104] 428g of kaolin and 1604g of decationized water were added to a slurrying tank, and the slurry was beaten for 60 minutes. Then, 286g of Hβ zeolite slurry (the slurry contained 167g of H (hydrogen type) β zeolite, and the solid content of the slurry was 35% by weight) was added, and stirred for 30 minutes. Finally, 227g of the large-particle sol (A1) obtained in the above Example 1 was added, and stirred for 15 minutes. The solid content of the obtained slurry was 19.7% by weight. The obtained slurry was then spray-dried and formed, and calcined at 500°C for 2 hours to obtain the catalytic cracking aid C1 containing the large-particle sol of the present invention.
[0105] Example 7
[0106] 349g of kaolin and 976g of decationized water were added to a slurrying tank, and the slurry was beaten for 60 minutes. Then, 289g of the large-particle sol (A2) obtained in Example 2 was added, and stirring was continued for 60 minutes. Finally, 329g of Hβ zeolite slurry (wherein the slurry contained 167g of Hβ zeolite and the solid content of the slurry was 38% by weight) was added, and stirring was continued for 30 minutes. The total solid content of the obtained slurry was 25.7% by weight. The obtained slurry was then spray-dried and formed, and calcined at 550°C for 1.5 hours to obtain the catalytic cracking aid C2 containing the large-particle sol of the present invention.
[0107] Example 8
[0108] 296g of kaolin, 403g of the large-particle sol (A3) obtained in Example 3 and 647g of decationized water were mixed and slurried, and stirred for 90 minutes; then 500g of Hβ zeolite slurry (wherein the slurry contained 200g of Hβ zeolite and the solid content of the slurry was 30% by weight) was added to the slurry, and stirred for 60 minutes, and the total solid content of the obtained slurry was 32.3% by weight. Then the obtained slurry was spray-dried and formed, and calcined at 600°C for 1.0h to obtain the catalytic cracking aid C3 containing the large-particle sol of the present invention.
[0109] Example 9
[0110] 543 g of Hβ zeolite slurry (including 253 g of Hβ zeolite and 35 wt% solid content) and 500 g of the large-particle sol (A4) obtained in Example 4 were mixed and stirred for 60 min; then 800 g of kaolin slurry (including 211 g of kaolin and 20 wt% solid content) was added to the slurry and stirred for 60 min. The solid content of the obtained slurry was 27.1 wt%. The obtained slurry was then spray-dried and calcined at 500° C. for 2 h to obtain the catalytic cracking aid C4 containing the large-particle sol of the present invention.
[0111] Example 10
[0112] 99g of kaolin and 276g of decationized water were added to a slurrying tank, slurrying was performed for 60 minutes, and then 643g of Hβ zeolite slurry (the slurry contained 300g of Hβ zeolite and the solid content of the slurry was 35% by weight) was added, stirred for 30 minutes, and finally 870g of the large-particle sol (A5) obtained in the above Example 5 was added, stirred for 30 minutes, and the solid content of the obtained slurry was 26.5% by weight. The obtained slurry was then spray-dried and formed, and calcined at 450°C for 2 hours to obtain the catalytic cracking aid C5 containing the large-particle sol of the present invention.
[0113] Comparative Examples 4 to 6
[0114] A catalytic cracking aid was prepared according to the method of Example 6, except that comparative examples 4 to 6 used the sol (DA1) prepared in comparative example 1, the sol (DA2) prepared in comparative example 2, and the sol (DA3) prepared in comparative example 3, respectively, instead of the large-particle sol (A1) prepared in example 1 used in example 6, to obtain comparative catalytic cracking aids DC1 to DC3 accordingly.
[0115] The physicochemical properties of the additives obtained in Examples 6 to 10 and Comparative Examples 4 to 6 are shown in Table 2. The pore size distribution of the additives is shown in Figure 3 .
[0116] Table 2 Composition and properties of catalytic cracking aids obtained in Examples 6 to 10 and Comparative Examples 4 to 6
[0117]
[0118] From Table 2 and Figure 3 It can be seen that compared with the comparative example, the total pore volume of the catalytic cracking aid containing large-particle sol prepared according to the method of the present invention is significantly increased, that is, it has a rich pore structure, and the proportion of 4-50nm mesopores is significantly increased, reaching more than 60% of the total pore volume.
[0119] The following Examples 11 to 15 and Comparative Examples 7 to 9 respectively evaluate the catalytic cracking performance and C4 olefin production increasing capability of the additives comprising the large particle size sol of the present invention and the comparative additives.
[0120] The additives C1-C5 containing large particle size sol prepared according to the method of the present invention, the additives DC1-DC3 prepared in the comparative example and the industrial catalyst (grade HSC, provided by Qilu Branch of Sinopec Catalyst Co., Ltd., main properties are shown in Table 3), are mixed into a catalyst mixture according to a mass ratio of 2:8, and the catalyst mixture is aged at 800°C and 100% water vapor for 17 hours on a fixed bed aging device. Then the evaluation is carried out on the ACE device, and the properties of the raw oil used for evaluation are shown in Table 4. The reaction temperature, catalyst-oil ratio, weight hourly space velocity and evaluation results are listed in Table 5. Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield; C4 olefin selectivity = C4 olefin yield / conversion rate.
[0121] Table 3 Properties of industrial catalysts
[0122]
[0123] Table 4 Raw oil properties
[0124]
[0125]
[0126] It can be seen from Table 5 that, compared with the comparative example, the catalytic cracking aid containing large particle size sol prepared in the embodiment of the present invention, when used in the catalytic cracking reaction of hydrocarbon oil, increases the yield of C4 olefins in the catalytic cracking reaction product, and significantly improves the selectivity of C4 olefins.
[0127] The present invention has been described above in conjunction with the preferred embodiments, which are merely exemplary and serve as an illustration. On this basis, the present invention may be subjected to a variety of substitutions and improvements, all of which fall within the scope of protection of the present invention.
Claims
1. A catalytic cracking aid comprising a large-particle sol, which comprises 15-50 wt% of beta zeolite, 10-75 wt% of clay, and 10-50 wt% of large-particle sol based on its dry weight; the large-particle sol comprises 10-40 wt% of Al2O3, 50-85 wt% of P2O5, and 0.2-10 wt% of SiO2 based on the dry weight of the large-particle sol, and the mass ratio of P2O5:Al2O3 is (1.5-5.0):1, and the mass ratio of SiO2:Al2O3 is (0.01-0.3):1, and the average particle size of the large-particle sol is in the range of 20-50 nm; the pore distribution is measured by a low-temperature nitrogen adsorption method, and the total pore volume of the catalytic cracking aid is not less than 0.200 mL / g, wherein the pore volume of mesopores with a pore size of 4-50 nm accounts for more than 60% of the total pore volume; The steps for preparing large particle size sol are as follows: (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25% by weight; (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the solid content of the obtained second slurry is 15 to 50% by weight; (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight; (1d) The third slurry is placed at 20-60° C. for 1-72 hours for aging treatment to obtain the large-particle sol.
2. The catalytic cracking aid according to claim 1, wherein the additive comprises 20 to 40% by weight of β zeolite, 20 to 65% by weight of clay and 15 to 45% by weight of large particle size sol, based on the total weight of the additive.
3. The catalytic cracking aid according to claim 2, wherein: The large-particle sol contains 15-35 wt% Al2O3, 55-80 wt% P2O5 and 0.5-8.0 wt% SiO2 on a dry basis, and the mass ratio of P2O5:Al2O is (2.0-4.5):1, and the mass ratio of SiO2:Al2O3 is (0.05-0.25):
1.
4. The catalytic cracking aid according to claim 1, wherein The average particle size of the large-particle sol is distributed in the range of 25 to 45 nm.
5. The catalytic cracking aid according to any one of claims 1 to 4, wherein The pore distribution is measured by low temperature nitrogen adsorption method, and the total pore volume of the catalytic cracking aid is 0.200-0.300 mL / g.
6. The catalytic cracking aid according to any one of claims 1 to 4, wherein The volume of mesopores with a pore diameter of 4 to 50 nm in the catalytic cracking aid accounts for 65 to 85% of the total pore volume.
7. The catalytic cracking aid according to claim 1, wherein The beta zeolite is selected from hydrogen beta zeolite, sodium beta zeolite, phosphorus and / or metal modified beta zeolite, metal modified beta zeolite or any combination thereof.
8. The catalytic cracking aid according to claim 1, wherein The beta zeolite is hydrogen beta zeolite, and the molar ratio of SiO2 to Al2O3 in the beta zeolite is 20-50; and the clay is selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite, and sepiolite.
9. The catalytic cracking aid according to claim 7, wherein The metal in the metal-modified beta zeolite is selected from one or more of La, Ce, Pr, Zr, Ti, Fe, Cu and Mg.
10. A method for preparing a catalytic cracking aid comprising a large particle size sol as claimed in any one of the preceding claims, comprising the following steps: (1) First, prepare a large particle size sol, the steps are as follows: (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25% by weight; (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the solid content of the obtained second slurry is 15 to 50% by weight; (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight; (1d) placing the third slurry at 20-60° C. for 1-72 hours for aging to obtain the large-particle sol; The mass ratio of the phosphorus source in terms of P2O5 to the aluminum source is (1.5-5.0):1, and the mass ratio of the silica sol in terms of SiO2 to the aluminum source in terms of Al2O3 is (0.01-0.3):
1. (2) Then, clay, β zeolite and the large particle size sol are uniformly mixed to obtain a slurry, wherein the solid content of the obtained slurry is 10-50% by weight, and the slurry is spray-dried, formed and calcined to obtain the aforementioned catalytic cracking aid, wherein, on a dry basis, the weight ratio of the β zeolite, the clay and the large particle size sol is (15-50):(10-75):(10-50).
11. The method according to claim 10, wherein: In step (1a), the mixing and stirring is performed for 30 to 60 minutes.
12. The method according to claim 10, wherein: Step (1b) is carried out at a temperature of 35-55° C., and the mixing and stirring is carried out for 30-90 minutes.
13. The method according to claim 10, wherein: Step (1c) is carried out at a temperature of 35-55° C., and the mixing and stirring is carried out for 30-90 minutes.
14. The method according to claim 10, wherein: The aluminum source is selected from one or more of pseudo-boehmite, alumina, boehmite, gibbsite and diaspore; the phosphorus source is selected from one or more of phosphoric acid, phosphorous acid and hypophosphorous acid; and the clay is selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.