A method for pre-lithiation of battery cell

By prelithiating lithium-ion batteries with lithium-liquid ammonia solution, the problems of battery cell damage and operation complexity in the existing technology are solved, and the efficient lithium replenishment and circulation performance of the battery are achieved, which is suitable for industrial applications.

CN115995620BActive Publication Date: 2024-11-15JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210586505.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-26
Publication Date
2024-11-15
Estimated Expiration
2042-05-26

AI Technical Summary

Technical Problem

The existing prelithiation technology of lithium-ion batteries has problems such as the generation of other substances that cause damage to the battery cell and complexity of operation, resulting in low safety and difficult to avoid damage to other materials.

Method used

The battery cell is prelithiated by using lithium-liquid ammonia solution. By mixing metal lithium with liquid ammonia and injecting it into the cooled battery cell, and prelithiating it during the heating process, the mole concentration and temperature of lithium can be controlled to achieve the Controlling lithium supplementation, simplifying operation and reducing environmental requirements.

Benefits of technology

It realizes efficient lithium replenishment of the battery cell, simplifies the operating process, reduces environmental requirements, avoids the damage of other substances to the battery cell, significantly improves the cycling performance and energy density of the battery, and can achieve industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115995620B_ABST
    Figure CN115995620B_ABST
Patent Text Reader

Abstract

The present invention provides a method for pre-lithiation of a battery cell, the method comprising the following steps: (1) mixing a metallic lithium source with liquid ammonia to obtain a lithium-liquid ammonia solution; (2) cooling the battery cell after the electrolyte is injected and allowing it to stand, and injecting the lithium-liquid ammonia solution obtained in step (1) into the cooled battery cell; (3) heating the battery cell injected with the lithium-liquid ammonia solution obtained in step (2) to obtain a pre-lithiation battery cell. The pre-lithiation method avoids damage caused by other materials in the battery during the pre-lithiation process, and the influence of other products generated during the pre-lithiation process on the battery cell. The pre-lithiation method is simple and has good effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a method for pre-lithiation of a battery cell. Background Art

[0002] In the first cycle of lithium-ion batteries, a SEI film is formed on the surface of the graphite negative electrode, resulting in an irreversible capacity loss of 5%-35%. This irreversible capacity greatly reduces the mass energy density and volume energy density of the battery. In order to compensate for the loss of irreversible capacity in the first cycle, people have studied pre-lithiation technology to improve the mass energy density and volume energy density of the battery. The pre-lithiation technology is used to replenish lithium in the electrode material so that the active lithium released during the charging process compensates for the irreversible lithium loss in the first cycle, thereby improving the reversible cycle capacity and cycle life of lithium-ion batteries.

[0003] CN113097451A discloses a pre-lithiation method, a pre-lithiation negative electrode sheet and a lithium-ion battery, comprising: 1) using a pre-lithiation agent to stir and pre-lithiate the negative electrode sheet to be pre-lithiated to obtain an intermediate pre-lithiated negative electrode sheet; 2) stirring, cleaning and drying the intermediate pre-lithiated negative electrode sheet in sequence to obtain a pre-lithiated negative electrode sheet; the stirring speed of the stirring pre-lithiation treatment and the stirring and cleaning treatment is 5 to 200 r / min, and the pre-lithiation agent includes a Li-polycyclic aromatic hydrocarbon methyl derivative. The pre-lithiation method needs to sacrifice other materials when replenishing lithium, and the products generated after the sacrifice of other materials have certain damage to the battery cell.

[0004] CN112786971A discloses a method for preparing a negative electrode pre-lithiation lithium ion battery: preparing a negative electrode plate, a positive electrode plate and a separator; compounding metal lithium to at least one surface of the negative electrode plate to obtain a composite negative electrode plate; assembling the composite negative electrode plate, the positive electrode plate and the separator into a bare battery cell, injecting electrolyte to obtain a lithium ion battery cell; subjecting the lithium ion battery cell to a positive and negative short circuit and a bidirectional pulse current treatment to accelerate the rapid and uniform diffusion of lithium ions and the formation of a negative electrode SEI film during the pre-lithiation process, and obtaining a negative electrode pre-lithiation lithium ion battery after formation. The method is complex, has relatively harsh environmental requirements, and is prone to safety accidents.

[0005] The above schemes have the problems of generating other substances that affect the battery cells or having low safety and complicated operation. Therefore, it is very necessary to develop a pre-lithiation method that is simple and safe to operate and can avoid generating other substances during the pre-lithiation process. Summary of the invention

[0006] The object of the present invention is to provide a method for pre-lithiation of a battery cell, which avoids damage to other materials in the battery during the pre-lithiation process and the influence of other products generated during the pre-lithiation process on the battery cell. The pre-lithiation method is simple and has good effect.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for pre-lithiation of a battery cell, the method comprising the following steps:

[0009] (1) mixing a metallic lithium source with liquid ammonia to obtain a lithium-liquid ammonia solution;

[0010] (2) cooling the battery cell after the electrolyte is injected and allowing it to stand, and injecting the lithium-liquid ammonia solution obtained in step (1) into the cooled battery cell;

[0011] (3) The battery cell injected with the lithium-liquid ammonia solution obtained in step (2) is heated to obtain a pre-lithiation battery cell.

[0012] The present invention replenishes lithium for the battery at the cell level, uses a lithium-liquid ammonia solution to directly pre-lithiate the cell, the pre-lithiation amount is controllable, the pre-lithiation method is simple, the requirements for the environment are low, the operation is easy, and industrialization can be realized.

[0013] The method of the present invention can not only be used to pre-lithiate lithium ion batteries, but also can be used to pre-sodium or pre-potassiumize sodium ion batteries or potassium ion batteries by replacing metallic lithium with metallic sodium or metallic potassium.

[0014] Preferably, the metallic lithium source in step (1) comprises lithium powder and / or lithium sheets.

[0015] Preferably, in the lithium-liquid ammonia solution of step (1), the molar concentration of lithium is 0.001-0.5 mol / L, for example: 0.001 mol / L, 0.005 mol / L, 0.01 mol / L, 0.03 mol / L, 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.3 mol / L or 0.5 mol / L, etc.

[0016] Preferably, in the lithium-liquid ammonia solution of step (1), the molar concentration of lithium is 0.03-0.08 mol / L, for example: 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L or 0.08 mol / L, etc.

[0017] Preferably, the standing temperature in step (2) is 20-30°C, for example, 20°C, 22°C, 25°C, 28°C or 30°C.

[0018] Preferably, the amount of electrolyte in the battery core is 3-5 g / Ah, for example: 3 g / Ah, 3.5 g / Ah, 4 g / Ah, 4.5 g / Ah or 5 g / Ah.

[0019] Preferably, the cooling temperature in step (2) is -33.5 to -56.6°C, for example: -33.5°C, -35°C, -40°C, -45°C, -50°C or -56.6°C, etc.

[0020] The present invention cools the electrolyte before pre-lithiation, which can prevent the lithium-liquid ammonia solution from contacting a high-temperature object and rapidly absorbing heat and gasifying, causing the lithium-liquid ammonia solution to splash out.

[0021] Preferably, the lithium content of the lithium-liquid ammonia solution injected in step (2) is 8-12% of the theoretical active lithium content of the battery cell, for example: 8%, 9%, 10%, 11% or 12%.

[0022] Preferably, the heating method in step (3) includes natural heating and / or temperature-controlled heating.

[0023] Preferably, the heating temperature is 20-30°C, for example, 20°C, 22°C, 25°C, 28°C or 30°C.

[0024] Preferably, the heating rate of the temperature-controlled heating is 0.1-5°C / min, for example, 0.1°C / min, 0.5°C / min, 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min.

[0025] Preferably, the heating is carried out under sealing conditions.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The present invention replenishes lithium for the battery at the cell level, and uses a lithium-liquid ammonia solution to directly pre-lithiate the cell. The amount of pre-lithiation is controllable, and the pre-lithiation method is simple, has low requirements on the environment, is easy to operate, and can be industrialized.

[0028] (2) The ammonia used in the pre-lithiation process of the present invention can be recycled and reused, thereby reducing resource waste and lowering carbon emissions.

[0029] (3) The capacity retention rate of the battery cell produced by the pre-lithiation method of the present invention after 500 cycles can reach more than 95.6%. By adjusting the pre-lithiation conditions, the capacity retention rate of the battery cell after 500 cycles can reach 99.8%. This shows that the pre-lithiation method of the present invention can supplement appropriate lithium to achieve a higher first-cycle coulombic efficiency while achieving a larger energy density and significantly improving the cycle performance of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic diagram of the pre-lithiation process described in Example 1-2 of the present invention, 1-lithium powder / lithium sheet, 2-liquid ammonia, 3-lithium-liquid ammonia solution, 4-battery cell, 5-pre-lithiation battery cell 5. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0032] Example 1

[0033] This embodiment provides a method for pre-lithiation of a battery cell, and the specific steps of the pre-lithiation method are as follows:

[0034] (1) Weighing 0.05 mol of lithium powder 1 and placing it into 1 L of liquid ammonia 2 to prepare a 0.05 mol / L lithium-liquid ammonia solution 3;

[0035] (2) cooling the battery cell 4 after the electrolyte is injected and allowed to stand at 25° C. to −45° C., and injecting the lithium-liquid ammonia solution 3 obtained in step (1) into the cooled battery cell 4, wherein the lithium content of the injected lithium-liquid ammonia solution is 10% of the theoretical active lithium content of the battery cell;

[0036] (3) The battery cell injected with the lithium-liquid ammonia solution obtained in step (2) is naturally heated to room temperature to obtain a pre-lithiation battery cell 5.

[0037] The schematic flow diagram of the pre-lithiation method is as follows Figure 1 shown.

[0038] Example 2

[0039] This embodiment provides a method for pre-lithiation of a battery cell, and the specific steps of the pre-lithiation method are as follows:

[0040] (1) Weighing 0.06 mol of lithium flakes 1 and placing them into 1 L of liquid ammonia 2 to prepare a 0.06 mol / L lithium-liquid ammonia solution 3;

[0041] (2) cooling the battery cell 4 after being injected with electrolyte and allowed to stand at 28° C. to −48° C., and injecting the lithium-liquid ammonia solution 3 obtained in step (1) into the cooled battery cell 4, wherein the lithium content of the injected lithium-liquid ammonia solution is 9% of the theoretical active lithium content of the battery cell;

[0042] (3) The battery cell injected with the lithium-liquid ammonia solution obtained in step (2) is heated to room temperature at a rate of 1° C. / min to obtain a pre-lithiation battery cell 5.

[0043] The schematic flow diagram of the pre-lithiation method is as follows Figure 1 shown.

[0044] Example 3

[0045] The only difference between this embodiment and embodiment 1 is that the concentration of the lithium-liquid ammonia solution in step (1) is 0.02 mol / L, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0046] Example 4

[0047] The only difference between this embodiment and embodiment 1 is that the concentration of the lithium-liquid ammonia solution in step (1) is 0.09 mol / L, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0048] Example 5

[0049] The only difference between this embodiment and embodiment 1 is that the lithium content of the lithium-liquid ammonia solution injected in step (2) is 6% of the theoretical active lithium content of the battery cell, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0050] Example 6

[0051] The only difference between this embodiment and embodiment 1 is that the lithium content of the lithium-liquid ammonia solution injected in step (2) is 15% of the theoretical active lithium content of the battery cell, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0052] Comparative Example 1

[0053] The only difference between this comparative example and Example 1 is that the negative electrode material is pre-lithiated with a lithium-liquid ammonia solution and then assembled into a battery cell.

[0054] Performance Testing:

[0055] The pre-lithiation cells obtained in Examples 1-6 and Comparative Example 1 were subjected to performance tests, and the test results are shown in Table 1:

[0056] Table 1

[0057]

[0058]

[0059] As can be seen from Table 1, from Examples 1-6, the capacity retention rate of the battery cell prepared by the pre-lithiation method of the present invention after 500 cycles can reach more than 95.6%, and by adjusting the pre-lithiation conditions, the capacity retention rate of the battery cell after 500 cycles can reach 99.8%, indicating that the pre-lithiation method of the present invention can supplement appropriate lithium to achieve a higher first-cycle coulombic efficiency while achieving a larger energy density and significantly improving the cycle performance of the battery cell.

[0060] By comparing Example 1 with Examples 3-4, it can be seen that the concentration of lithium in the lithium-liquid ammonia solution in step (1) affects the effect of pre-lithiation. When the concentration of lithium in the lithium-liquid ammonia solution is controlled at 0.03-0.08 mol / L, the effect of pre-lithiation is better. If the concentration of lithium in the lithium-liquid ammonia solution is too low, the injection volume is too large, which increases the difficulty of operation and leads to slow physical and chemical rate. When the temperature is increased, the lithium-liquid ammonia solution overflows. If the concentration of lithium in the lithium-liquid ammonia solution is too high, the physical and chemical rate is faster, the current is larger, and the impact on the material is greater. Although a higher first-cycle coulomb efficiency can be obtained, the cycle performance is reduced.

[0061] By comparing Example 1 with Examples 5-6, it can be seen that the amount of lithium-liquid ammonia solution injected in step (2) will affect the effect of pre-lithiation. The pre-lithiation effect is better when the lithium content of the injected lithium-liquid ammonia solution is controlled at 8-12% of the theoretical active lithium content of the battery cell. If the amount of lithium-liquid ammonia solution injected is too much, more lithium is supplemented, the battery is prone to lithium precipitation, and the cycle performance decreases rapidly. If the amount of lithium-liquid ammonia solution injected is too little, the first-cycle coulomb efficiency is not high, the battery energy density decreases, and the cycle performance decreases.

[0062] By comparing Example 1 and Comparative Example 1, it can be seen that the present invention uses a lithium-liquid ammonia solution to directly pre-lithiate the battery cell. The pre-lithiation method is simple and can avoid damage to other materials in the battery during the pre-lithiation process and the influence of other products on the battery cell, and the pre-lithiation effect is significantly improved.

[0063] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for pre-lithiation of a battery cell, characterized in that: The pre-lithiation method comprises the following steps: (1) mixing a metallic lithium source with liquid ammonia to obtain a lithium-liquid ammonia solution; In the lithium-liquid ammonia solution of step (1), the molar concentration of lithium is 0.03-0.08 mol / L; (2) cooling the battery cell after the electrolyte is injected and allowing it to stand, and injecting the lithium-liquid ammonia solution obtained in step (1) into the cooled battery cell; The lithium content of the lithium-liquid ammonia solution injected in step (2) is 8-12% of the theoretical active lithium content of the battery cell; (3) The battery cell injected with the lithium-liquid ammonia solution obtained in step (2) is heated to obtain a pre-lithiation battery cell.

2. The method according to claim 1, characterized in that The metallic lithium source in step (1) includes lithium powder and / or lithium flakes.

3. The method according to claim 1, characterized in that The standing temperature in step (2) is 20-30°C.

4. The method according to claim 1, characterized in that The amount of electrolyte in the battery cell in step (2) is 3-5 g / Ah.

5. The method according to claim 1, characterized in that The cooling temperature is -33.5~-56.6℃.

6. The method according to claim 1, characterized in that The heating method in step (3) includes natural heating and / or temperature-controlled heating.

7. The method according to claim 1, characterized in that The temperature of the heating in step (3) is 20-30°C.

8. The method according to claim 6, characterized in that The heating rate of the temperature-controlled heating is 0.1-5°C / min.

9. The method according to claim 1, characterized in that The temperature increase is performed under a sealing condition.