A porous ammonia synthesis catalyst and its preparation method and application
The preparation of porous metal silicate catalysts by sol-gel method solves the problems of high energy consumption and poor stability of existing ammonia synthesis catalysts under high temperature and high pressure, and achieves efficient catalytic ammonia synthesis under low temperature and low pressure conditions, reducing energy consumption And improves the stability and cost-effectiveness of the catalyst.
Patent Information
- Application Number
- CN202310020399.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-01-06
AI Technical Summary
The existing ammonia synthesis catalysts have problems such as high energy consumption, serious pollution and poor catalyst stability under high temperature and high pressure conditions. Moreover, the preparation cost of ruthenium-based catalysts is high, making it difficult to efficiently catalyze ammonia synthesis under mild conditions.
The porous ammonia synthesis catalyst is prepared by sol-gel method, and the porous metal silicate catalyst is formed through hydrothermal reaction between metal complexes and silicon sources, and the iron active center is introduced and cocatalytic elements are doped to form a high specific surface area and uniform pore channels. Distributed catalyst, suitable for ammonia synthesis under low temperature and low pressure conditions.
It realizes efficient catalytic ammonia synthesis under low temperature and low pressure conditions, reduces energy consumption, improves the stability and cost-effectiveness of the catalyst, solves the problems of high energy consumption and pollution of traditional catalysts, and has important industrial application prospects.
Smart Images

Figure CN115999550B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation of ammonia synthesis catalysts, and in particular to a porous ammonia synthesis catalyst and a preparation method and application thereof. Background Art
[0002] Ammonia is one of the most important raw materials for synthetic chemical products and fertilizers, and has great application prospects in the field of hydrogen storage in recent years. In 1904, Haber first used an iron-based catalyst to prepare ammonia with hydrogen and nitrogen as raw materials under high temperature and high pressure conditions, and Bosch realized industrialization in 1913. Since then, research on synthetic ammonia has received widespread attention and has developed rapidly. Almquist et al. studied the relationship between the activity of pure iron catalysts and iron components with different valence states, and confirmed that Fe3O4-based catalysts have the highest activity; Bridger et al. found that the introduction of Al2O3-K2O dual additives can greatly improve the catalytic activity of iron-based catalysts; in 1979, the British Imperial Chemical Industries Group took the lead in using cobalt oxide as an additive to develop Fe2Co catalysts, which further improved the catalytic activity; in 1985, Liu Huazhang et al. found that Fe with a wustite structure 1-x O-based catalysts have higher catalytic activity for ammonia synthesis and have been industrialized. In 1992, British Petroleum and Kellogg Company of the United States jointly developed the first ruthenium-based catalyst and its process flow (KAAP), which is considered to be the second-generation ammonia synthesis catalyst.
[0003] The iron-based catalyst used for industrial ammonia synthesis is prepared by melting Fe3O4 with different types of promoters (Al2O3, CaO, K2O, etc.) at a temperature of about 2000K. The ammonia synthesis process needs to be carried out under high temperature (400-600℃) and high pressure (10-30MPa). It has the disadvantages of high energy consumption (accounting for 1%-2% of the world's annual energy) and emission of a large amount of greenhouse gases (such as CO2). The harsh reaction conditions will also cause serious sintering of the catalyst and loss of active sites. Ruthenium-based catalysts have poor stability (easy to sinter and aggregate under high temperature conditions, easy to be poisoned by hydrogen), and have a higher preparation cost than cheap transition metals. Therefore, the development of a new catalyst that is low-cost, environmentally friendly, energy-saving, more stable, and can achieve ammonia synthesis under mild conditions has become an important research topic in today's era. Summary of the invention
[0004] The purpose of the present invention is to provide a porous ammonia synthesis catalyst, a preparation method and a use thereof, in view of the problems existing in the existing ammonia synthesis catalysts, which can realize efficient catalytic ammonia synthesis under low temperature and low pressure conditions and has the application prospect of replacing the existing industrial ammonia synthesis catalysts.
[0005] The technical solution adopted by the present invention is:
[0006] A porous ammonia synthesis catalyst is prepared by a sol-gel method using a metal complex as a template and a silicon source as a raw material; the metal complex is a compound formed by a metal ion and an organic ligand through a coordination bond; the metal ion is composed of one or more of boron, aluminum, zirconium, nickel, titanium, cobalt, manganese, vanadium, chromium, iron, copper, zinc, tungsten, platinum, ruthenium, rhodium, palladium, lanthanum, cerium, praseodymium, samarium, neodymium, dysprosium, cesium, sodium, potassium, magnesium, calcium, and barium ions mixed in a proportion; the organic ligand is an organic compound composed of two or more elements selected from nitrogen, phosphorus, and oxygen atoms mixed in a proportion.
[0007] Furthermore, the organic ligand is preferably a carboxylic acid ligand, and the carboxylic acid ligand is preferably one or more of benzoic acid, pyridinecarboxylic acid, terephthalic acid, formic acid, acetic acid, propionic acid, 1-naphthoic acid, and 2-naphthoic acid.
[0008] Furthermore, the silicon source is preferably a silicate or sodium metasilicate; the silicate is preferably one or more of methyl orthosilicate, tetraethyl orthosilicate, tetrabutyl orthosilicate, and tetraisopropyl orthosilicate.
[0009] Furthermore, the porous ammonia synthesis catalyst is a silicate catalytic material containing metal active centers, and the molar ratio of silicon to metal active centers is 2 to 100:1.
[0010] Furthermore, the specific surface area of the porous ammonia synthesis catalyst is 50 to 800 m 2 / g, pore size is 1 to 10 nm.
[0011] Furthermore, the porous ammonia synthesis catalyst is an iron-based catalyst, the metal ions are composed of iron ions and other catalytic promoter ions mixed in a ratio; the other catalytic promoter ions are one or more of boron, sodium, potassium, magnesium, calcium, barium, cesium, aluminum, zirconium, nickel, titanium, cobalt, manganese, vanadium, chromium, copper, zinc, tungsten, platinum, ruthenium, rhodium, palladium, lanthanum, cerium, praseodymium, samarium, neodymium, and dysprosium ions. By in-situ introduction of iron active centers in the porous metal silicate material and by doping with different catalytic promoter elements, the catalytic efficiency of the catalyst is greatly improved.
[0012] A method for preparing the porous ammonia synthesis catalyst adopts a sol-gel method, comprising the following steps: adding a silicon source to a metal carboxylate solution, stirring until fully dissolved, placing the solution in a hydrothermal reaction kettle, placing the solution in an oven for hydrothermal reaction to form a gel, drying the solution, transferring the solution to a muffle furnace, heating the solution to 100-1000° C. in an air atmosphere, and calcining the solution at a constant temperature for 1-24 hours; or placing the solution in a tubular furnace, heating the solution to 100-1000° C. in an inert atmosphere, and calcining the solution at a constant temperature for 1-24 hours, thereby obtaining a porous ammonia synthesis catalyst.
[0013] Furthermore, the metal carboxylate solution is prepared by dissolving a carboxylic acid ligand and a metal salt in a solvent at a molar ratio of 0.5 to 10:1; the metal ions in the metal salt are composed of one or more of boron, sodium, potassium, magnesium, calcium, barium, cesium, aluminum, zirconium, nickel, titanium, cobalt, manganese, vanadium, chromium, iron, copper, zinc, tungsten, platinum, ruthenium, rhodium, palladium, lanthanum, cerium, praseodymium, samarium, neodymium, and dysprosium ions mixed in a proportion; and the solvent is one or more of water, methanol, ethanol, N,N-dimethylformamide, acetonitrile, and acetone mixed in any proportion.
[0014] Furthermore, the metal carboxylate is preferably a benzoate, and the metal salt is dissolved in the solvent in a molar ratio of 1-5:0.5-1.
[0015] Furthermore, the concentration of metal ions in the metal carboxylate solution is 0.1-1 mmol / L.
[0016] Furthermore, the metal salt is a substance soluble in a solvent, such as chloride, nitrate, acetate, sulfate, etc.
[0017] Furthermore, the conditions of the hydrothermal reaction are: 80°C to 200°C, 6h to 48h.
[0018] An application of the porous ammonia synthesis catalyst in ammonia synthesis reaction.
[0019] Furthermore, the specific operation is as follows: the porous ammonia synthesis catalyst is mixed with quartz sand and loaded into a reactor, the reaction gas is a nitrogen-hydrogen mixed gas, the nitrogen-hydrogen ratio is 0.1-10:1, the reaction conditions are 0.1-15MPa, the reaction temperature is 150-450°C, and the reaction space velocity is 1-72L·g -1 ·h -1 .
[0020] Compared with the prior art, the present invention has the following effects:
[0021] 1. The porous ammonia synthesis catalyst of the present invention has low preparation cost, simple process and no pollution;
[0022] 2. The pore size of the porous ammonia synthesis catalyst can be controlled by adjusting the ratio of silicon to metal ions, the composition of metal ions, etc., with a large specific surface area and uniform pore distribution;
[0023] 3. The active metal components, structure, particle size, distribution, etc. of the porous ammonia synthesis catalyst can be adjusted by adjusting the ratio of silicon to metal ions, which is easy to control and the aggregation degree of metal active centers can be easily adjusted, thereby improving the catalytic efficiency;
[0024] 4. When the porous ammonia synthesis catalyst is used to catalyze the ammonia synthesis reaction, the reaction temperature and pressure are low, the energy consumption is low, the catalytic efficiency is high, the stability is high, and it is environmentally friendly. It can solve the high energy consumption and pollution problems of traditional industrial catalysts and has important industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a graph showing the results of catalytic synthesis of ammonia by PMS-100, PMS-100-a and DNCA ammonia synthesis catalysts at a pressure of 2MPa and different temperatures. DETAILED DESCRIPTION
[0026] The invention discloses a porous ammonia synthesis catalyst and a preparation method and use thereof. The porous ammonia synthesis catalyst uses a porous metal silicate as a skeleton and one or more metals in proportion to form a catalytic active center. The raw material cost is low, the catalyst is easy to prepare, and the energy consumption is low. When the porous ammonia synthesis catalyst is used for catalytic synthesis of ammonia, the reaction pressure and temperature are low, the catalytic efficiency is high, the energy consumption is low, there is no pollution, and the catalyst can be used for a long time with high activity.
[0027] The following examples will help to understand the present invention, but the protection scope of the present invention is not limited to these contents:
[0028] Example 1
[0029] Benzoic acid (13.44mmol), ferric nitrate (2.24mmol), cesium chloride (0.112mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120℃ for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor and aged at 160℃ for 24h to form a gel. The dried solid of the gel was transferred to a muffle furnace and calcined at 600℃ in an air atmosphere for 5 hours to obtain a solid material named PMS-100. The specific surface area of the porous ammonia synthesis catalyst is 427m 2 / g, the pores are evenly distributed and the average pore size is 0.96nm.
[0030] Example 2
[0031] Benzoic acid (13.44mmol), ferric nitrate (2.24mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120℃ for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor and aged at 160℃ for 24h to form a gel. The dried solid was transferred to a muffle furnace and calcined at 600℃ in an air atmosphere for 5 hours to obtain a solid material named PMS-100-a. The specific surface area of the porous ammonia synthesis catalyst is 475m2 / g, the pores are evenly distributed and the average pore size is 0.83nm.
[0032] Example 3
[0033] Benzoic acid (13.44mmol), ferric nitrate (2.24mmol), calcium chloride (0.112mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120℃ for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor and aged at 160℃ for 24h to form a gel. The dried solid was transferred to a muffle furnace and calcined at 600℃ in an air atmosphere to obtain a solid material named PMS-100-b. The specific surface area of the porous ammonia synthesis catalyst is 456m 2 / g, the pore distribution is uniform, and the average pore size is 0.90nm.
[0034] Example 4
[0035] Benzoic acid (13.44mmol), ferric nitrate (2.24mmol), boric acid (0.112mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor and aged at 160°C for 24h to form a gel. The dried solid was transferred to a muffle furnace and calcined at 600°C in an air atmosphere to obtain a solid material, named PMS-100-c. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above-mentioned embodiment.
[0036] Example 5
[0037] Benzoic acid (13.44mmol), ferric nitrate (2.24mmol), aluminum chloride (0.112mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor and aged at 160°C for 24h to form a gel. The dried solid was transferred to a muffle furnace and calcined at 600°C in an air atmosphere to obtain a solid material named PMS-100-d. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above-mentioned embodiment.
[0038] Example 6
[0039] Benzoic acid (13.44mmol), ferric nitrate (2.24mmol), aluminum chloride (0.112mmol), potassium nitrate (0.224mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor, aged at 160°C for 24h to form a gel, and the dried solid was transferred to a muffle furnace and calcined at 600°C in an air atmosphere to obtain a solid material, named PMS-100-e. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above embodiment.
[0040] Example 7
[0041] Benzoic acid (13.44mmol), ferric nitrate (2.24mmol), chromium nitrate (0.112mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor and aged at 160°C for 24h to form a gel. The dried solid was transferred to a muffle furnace and calcined at 600°C in an air atmosphere to obtain a solid material named PMS-100-f. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above-mentioned embodiment.
[0042] Example 8
[0043] Benzoic acid (13.44mmol), ferric nitrate (2.24mmol), cerium chloride (0.112mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor and aged at 160°C for 24h to form a gel. The dried solid was transferred to a muffle furnace and calcined at 600°C in an air atmosphere to obtain a solid material, named PMS-100-g. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above-mentioned embodiment.
[0044] Example 9
[0045] The activity evaluation of the catalyst was carried out in a high-pressure activity test device with an inner diameter of 8 mm. The catalysts prepared in Examples 1-8 or commercial catalysts (specific usage amounts are shown in Table 1) were mixed with a certain amount of quartz sand and loaded into a stainless steel reactor. The reaction gas was a nitrogen-hydrogen mixed gas with a nitrogen-hydrogen ratio of 1:3, the reaction pressure was 2 MPa, the reaction temperature was 350°C, and the reaction space velocity was 9 L·g -1 ·h -1 The reaction gas was absorbed by dilute sulfuric acid aqueous solution, and the ammonium ion concentration in the absorption liquid was determined by ion chromatography. The results are shown in Table 1. Under the same conditions, when the catalyst of the present invention is used to catalyze ammonia synthesis, the catalytic efficiency is much higher than that of the DNCA type industrial ammonia synthesis catalyst and the commercial ruthenium carbon catalyst, indicating that the present invention has good industrial application prospects.
[0046] Table 1 Comparison table of synthetic ammonia performance test results of Examples 1 to 10, Comparative Example 1 and Comparative Example 2
[0047]
[0048] Example 10
[0049] 0.2 g of PMS-100 / PMS-100-a / DNCA was mixed with a certain amount of quartz sand and loaded into a stainless steel reactor. The reaction gas was nitrogen-hydrogen mixed gas with a nitrogen-hydrogen ratio of 1:3. The reaction pressure was 2 MPa. The reaction temperature was increased from 250°C to 400°C at 25°C intervals. The reaction space velocity was 9 L·g -1 ·h -1 At each temperature, the reaction gas was absorbed by dilute sulfuric acid aqueous solution, and the ammonium ion concentration in the absorption liquid was determined by ion chromatography. Figure 1 As shown, it is explained that the catalytic efficiency of the catalyst of the present invention is much higher than that of the DNCA type industrial ammonia synthesis catalyst.
[0050] Embodiment 11
[0051] Benzoic acid (26.88mmol), ferric nitrate (4.48mmol), cobalt nitrate (0.112mmol) and tetraethyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor, aged at 100°C for 12h to form a gel, and the dried solid was transferred to a muffle furnace and calcined at 400°C in an air atmosphere for 8h to obtain a solid material. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above embodiment, and has good ammonia synthesis catalytic efficiency.
[0052] Example 12
[0053] Formic acid (13.44mmol), platinum nitrate (1.344mmol) and methyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor, aged at 120°C for 16h to form a gel, and the dried solid of the gel was transferred to a muffle furnace and calcined at 100°C in an air atmosphere for 24 hours to obtain a solid material. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above embodiment, and has good ammonia synthesis catalytic efficiency.
[0054] Embodiment 13
[0055] Acetic acid (1.12 mmol), cobalt nitrate (2.24 mmol) and sodium metasilicate (6.72 mmol) were added to 4 mL of water, stirred at 100° C. for 4 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor, aged at 200° C. for 20 hours to form a gel, and the dried solid of the gel was transferred to a tubular furnace and calcined at 600° C. for 1 hour in a nitrogen atmosphere to obtain a solid material. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above-mentioned embodiment, and has good ammonia synthesis catalytic efficiency.
[0056] Embodiment 14
[0057] Terephthalic acid (13.44mmol), rhodium chloride (2.24mmol), cesium chloride (0.112mmol) and chlorosilane (235.2mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor, aged at 160°C for 36h to form a gel, and the dried solid of the gel was transferred to a muffle furnace and calcined at 600°C in an air atmosphere for 4.5 hours to obtain a solid material. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above embodiment, and has good ammonia synthesis catalytic efficiency.
[0058] Embodiment 15
[0059] 1-Naphthoic acid (13.44mmol), ferric nitrate (2.24mmol), cerium chloride (0.112mmol) and tetraisopropyl orthosilicate (6.72mmol) were added to a mixed solvent of 4mL N,N-dimethylformamide and 0.5mL water, stirred at 120°C for 3 hours, cooled to room temperature and stirred overnight. The mixed solution was placed in a hydrothermal reactor and aged at 200°C for 48h to form a gel. The dried solid of the gel was transferred to a muffle furnace and calcined at 600°C in an air atmosphere for 5 hours to obtain a solid material. The porous ammonia synthesis catalyst has uniform pore distribution, and the specific surface area and average pore size have similar characteristics to the materials in the above embodiment, and has good ammonia synthesis catalytic efficiency.
[0060] The above descriptions are only some embodiments of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention are within the scope of the present invention.
Claims
1. Application of a porous ammonia synthesis catalyst in ammonia synthesis reaction, characterized in that: The porous ammonia synthesis catalyst is a silicate catalytic material containing a metal active center, which is prepared by a sol-gel method using a metal complex as a template and a silicon source as a raw material; the metal complex is a compound formed by a metal ion and an organic ligand through a coordination bond; the metal ion is composed of a mixture of iron ions and other catalytic promoter element ions in a proportion; the other catalytic promoter element ions are one or more of boron, sodium, potassium, magnesium, calcium, barium, cesium, aluminum, zirconium, nickel, titanium, cobalt, manganese, vanadium, chromium, copper, zinc, tungsten, platinum, ruthenium, rhodium, palladium, lanthanum, cerium, praseodymium, samarium, neodymium, and dysprosium ions; the organic ligand is an organic compound containing one or more of nitrogen, phosphorus, and oxygen atoms, and the organic ligand is a carboxylic acid ligand.
2. The use according to claim 1, characterized in that: The carboxylic acid ligand is one or more of benzoic acid, pyridinecarboxylic acid, terephthalic acid, formic acid, acetic acid, propionic acid, 1-naphthoic acid and 2-naphthoic acid.
3. The use according to claim 1, characterized in that: The silicon source is silicate, sodium metasilicate, and chlorosilane; the silicate is one or more of methyl orthosilicate, tetraethyl orthosilicate, tetrabutyl orthosilicate, and tetraisopropyl orthosilicate.
4. The use according to claim 1, characterized in that: In the silicate catalytic material containing metal active centers, the molar ratio of silicon to metal active centers is 2:1 to 100:
1.
5. The use according to claim 1, characterized in that: The specific surface area of the porous ammonia synthesis catalyst is 50-800 m 2 / g, pore size is 1~10 nm.
6. The use according to claim 1, characterized in that: The porous ammonia synthesis catalyst is prepared by the following method: adding a silicon source to a metal carboxylate solution, placing the solution in a hydrothermal reactor after fully dissolving the solution, placing the solution in an oven for hydrothermal reaction to form a gel, drying the gel, transferring the gel to a muffle furnace, and heating the solution to a temperature of 100 to 1000°C in an air atmosphere. o C, calcine at a constant temperature for 1-24 h; or place the dried gel in a tube furnace and heat to 100-1000 C in an inert atmosphere. o C, calcined at constant temperature for 1 to 24 h to obtain a porous ammonia synthesis catalyst.
7. The use according to claim 6, characterized in that: The metal carboxylate solution is prepared by dissolving a carboxylic acid ligand and a metal salt in a solvent at a molar ratio of 0.5 to 10:1; the metal ions in the metal salt are composed of iron ions and other catalytic promoter element ions mixed in a proportion; the other catalytic promoter element ions are one or more of boron, sodium, potassium, magnesium, calcium, barium, cesium, aluminum, zirconium, nickel, titanium, cobalt, manganese, vanadium, chromium, copper, zinc, tungsten, platinum, ruthenium, rhodium, palladium, lanthanum, cerium, praseodymium, samarium, neodymium, and dysprosium ions; and the solvent is one or more of water, methanol, ethanol, N,N-dimethylformamide, acetonitrile, and acetone mixed in any proportion.