A naphtha catalytic reforming catalyst and preparation method thereof
By using alumina support and impregnation method containing sulfate and phosphate, the structure and performance of the platinum rhenium catalyst are optimized, and the problems of hydrogenolysis reaction and sulfate toxicity of the platinum rhenium catalyst during operation are solved, achieving high activity and long-term Lifespan and highly selective catalytic effects.
Patent Information
- Application Number
- CN202111228864.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-21
AI Technical Summary
The existing platinum-rhenium reforming catalysts are prone to strong hydrogenolysis reactions when starting construction, resulting in rapid increase in the temperature of the catalyst bed, causing carbon accumulation and activity damage, and sulfate is harmful to the performance of the catalyst, affecting service life and selectivity.
Using alumina containing sulfate and phosphate as a carrier, the pore distribution is optimized by high-temperature water vapor treatment, and the active metal components are loaded to reduce the ring opening reaction, improve the selectivity of the cyclization reaction, and indium or yttrium is introduced through the impregnation method to Improve catalyst performance.
The high activity and stability of the catalyst are achieved, the aromatizing activity and selectivity are improved, the service life is extended, the construction start steps are simplified, and the toxic effects of sulfate are effectively reduced.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0003315236570000021
Abstract
Description
Technical Field
[0001] The present invention relates to a hydrocarbon conversion catalyst and a preparation method thereof, in particular to a naphtha reforming catalyst and a preparation method thereof. Background Art
[0002] Catalytic reforming is based on C6~C 12 The process of using naphtha fractions of crude oil as raw materials, and causing the raw hydrocarbon molecules to undergo reforming reactions such as cycloalkane dehydrogenation, linear alkane dehydrogenation isomerization, and chain alkane dehydrogenation cyclization under certain temperature, pressure, hydrogen and catalyst to produce high-octane gasoline blending components or aromatics, and produce cheap hydrogen as a by-product. At present, the supported bifunctional reforming catalyst widely used in catalytic reforming processes includes hydrogenation / dehydrogenation functions provided by metal components and acidic isomerization functions provided by carriers. Reforming catalysts are usually bimetallic (multimetallic) catalysts with activated alumina as carrier, Pt as the main metal component, and a second metal component such as rhenium, tin or germanium.
[0003] Catalysts are the core of reforming technology. Current research on the development of reforming catalysts shows that to improve the reaction performance of catalysts, it is necessary to first develop a carrier with excellent performance. For an ideal carrier, it is necessary to increase efforts in carrier raw materials, preparation methods and modified components to achieve physical and chemical properties such as low impurity content, suitable and stable crystal structure, good hydrothermal stability, suitable acidity, good mass transfer and heat transfer performance, and mechanical strength.
[0004] For platinum-rhenium reforming catalysts, since metallic rhenium has a high hydrogenolysis activity, if the activity of rhenium is not passivated at the start of operation, a strong hydrogenolysis reaction will occur at the initial stage of oil inflow, releasing a large amount of reaction heat, causing the catalyst bed temperature to rise rapidly and overheating. Once this phenomenon occurs, it often causes serious consequences. At the very least, it causes a large amount of carbon deposition on the catalyst, which damages the activity and stability of the catalyst, and at the worst, it burns the catalyst, reactor and internal components. Therefore, the platinum-rhenium reforming catalyst used in industrial equipment needs to be pre-sulfurized before use. Through pre-sulfurization, the excessive hydrogenolysis reaction of the fresh catalyst is suppressed to protect the activity and stability of the catalyst and improve the selectivity of the catalyst.
[0005] It is generally believed that sulfate in the reforming catalyst will damage the performance of the catalyst and is a poison to the catalyst. CN98117895.2 discloses a method for removing sulfate from the reforming catalyst, which is to introduce an organic chlorine compound that decomposes hydrogen chloride under the condition into the catalyst bed poisoned by sulfate at 400-600°C to remove the sulfate. Compared with conventional catalyst chlorination and regeneration, this method can effectively remove sulfate from the catalyst.
[0006] CN102139222A discloses a platinum-rhenium reforming catalyst, which contains 0.1-0.3% by mass of sulfate. The sulfate is introduced by co-impregnation or sub-impregnation during the catalyst preparation process, and the obtained catalyst can be used for catalytic reforming reaction without pre-sulfurization. The catalyst has a long service life and good catalytic performance, and the start-up steps are simplified. Summary of the invention
[0007] The object of the present invention is to provide a naphtha catalytic reforming catalyst and a preparation method thereof. The catalyst is used for naphtha catalytic reforming reaction and has high aromatization activity and selectivity.
[0008] The naphtha catalytic reforming catalyst provided by the present invention comprises an alumina carrier containing sulfate and phosphate and components having the following contents based on the alumina:
[0009]
[0010] The invention uses alumina containing sulfate and phosphate as a carrier and then loads active components to prepare a catalyst for naphtha catalytic reforming reaction, and has high aromatization activity and selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 This is a spherical aberration corrected scanning transmission electron microscope (AC-STEM) image of the catalyst prepared in Example 3 of the present invention.
[0012] Figure 2 This is a spherical aberration corrected scanning transmission electron microscopy image of the catalyst prepared in Comparative Example 5. DETAILED DESCRIPTION
[0013] The aluminum oxide carrier containing sulfate and phosphate described in the present invention is formed from aluminum hydroxide containing sulfate and phosphate and then treated with high-temperature steam. It has a more ideal pore distribution. The loaded active metal components interact with the sulfate and phosphate in the carrier, which can reasonably optimize the acidity of the carrier, promote the dehydrogenation cyclization of alkanes, reduce the ring-opening reaction, and further improve the selectivity of the cyclization reaction relative to the cracking reaction, so that the catalyst has both high activity and high stability, thereby improving the liquid yield and aromatics yield of the reaction.
[0014] Preferably, the catalyst comprises the following components:
[0015]
[0016] The sulfate- and phosphate-containing alumina carrier of the present invention is preferably γ-alumina containing sulfate and phosphate. Preferably, the sulfate- and phosphate-containing alumina carrier is made from aluminum hydroxide containing sulfate and phosphate, and the sodium content in the carrier based on alumina is preferably 0.008 to 0.02% by mass.
[0017] The sulfate- and phosphate-containing alumina carrier of the present invention preferably has the following pore diameter distribution: pores with a pore diameter of 4 to 6 nm account for 4 to 6% by volume of the total pore volume, pores with a pore diameter of 6 to 10 nm account for 86 to 90% by volume of the total pore volume, more preferably 86 to 88% by volume, pores with a pore diameter of 10 to 20 nm account for 5 to 7% by volume of the total pore volume, and pores with a pore diameter greater than 20 nm account for 1 to 3% by volume of the total pore volume.
[0018] The catalyst of the present invention may further include 0.05 to 3.0 mass %, preferably 0.05 to 1.0 mass % of indium or yttrium.
[0019] The Group VIII metal of the present invention is preferably platinum, the Group VIIB metal is preferably rhenium, and the halogen is preferably chlorine.
[0020] The specific surface area of the alumina carrier containing sulfate and phosphate is preferably 190 to 220 m 2 / g, and the pore volume is preferably 0.4 to 0.7 mL / g.
[0021] The preparation method of the catalyst of the present invention comprises the steps of impregnating an aluminum oxide carrier containing sulfate and phosphate with a solution containing a Group VIII metal compound, a Group VIIB metal compound and a halogen as an impregnation liquid, and drying and calcining the impregnated solid.
[0022] In the above preparation method, the impregnation solution further contains an indium or yttrium compound, and the indium or yttrium compound is preferably an indium or yttrium nitrate or chloride. The indium or yttrium can also be introduced into the carrier by a fractional leaching method, that is, the carrier is first impregnated with a solution containing an indium or yttrium compound as an impregnation solution, and then the carrier containing sulfate is impregnated with a solution containing a Group VIII metal compound, a Group VIIB metal compound and a halogen as an impregnation solution, and the impregnated solid is dried and calcined.
[0023] In the above preparation method, the Group VIII metal compound is selected from chloroplatinic acid, tetraammonium dichloroplatinum, ammonium chloroplatinate, platinum trichloride, platinum tetrachloride hydrate, dicarbonyl platinum dichloride, dinitrodiaminoplatinum or sodium tetranitroplatinate, preferably chloroplatinic acid; the Group VIIB metal compound is selected from perrhenic acid or ammonium perrhenate; the halogen is preferably chlorine.
[0024] In order to make the Group VIII metal more uniformly distributed on the support, the impregnation solution for impregnating the Group VIII metal compound preferably contains hydrochloric acid.
[0025] In the above method, the method of introducing active components by impregnation can be saturated impregnation or supersaturated impregnation. During saturated impregnation, the liquid / solid volume ratio of the impregnation solution to the carrier is less than 1.0, preferably 0.5-0.9, and the impregnation solution is completely absorbed by the carrier. The liquid / solid volume ratio of the impregnation solution used for supersaturated impregnation to the carrier is greater than 1.0, preferably 1.1-3.0. After impregnation, the excess impregnation solution is removed by filtering or vacuum evaporation of the solvent. The vacuum evaporation method of the solvent can be carried out using a rotary vacuum evaporator. The specific operation method is: prepare the water-soluble compound containing each active component into an impregnation solution, impregnate the aluminum oxide containing sulfate and phosphate under the conditions of 0.001-0.10MPa and rotation, the liquid / solid volume ratio of the impregnation solution to the aluminum oxide containing sulfate and phosphate is 1.1-3.0, the rotation line speed is 0.01-2.0 m / s, and after impregnation, it is dried and calcined for activation. The pressure of vacuum rotary impregnation is preferably 0.001-0.08 MPa. During impregnation, the catalyst is heated and rotated at the same time. The heating temperature, i.e., the impregnation temperature, is preferably 20-60°C, more preferably 20-40°C. The rotation rate should not be too fast. The preferred rotation linear speed is 0.02-0.8 m / s, more preferably 0.03-0.5 m / s. The impregnation time is preferably 1-8 hours, more preferably 2-4 hours. After vacuum rotary impregnation, the water in the impregnation liquid has been basically evaporated, and the catalyst is in a dry state. At this time, the carrier can be directly taken out for drying and calcination.
[0026] In the above method, the drying temperature of the solid obtained after the active component is introduced by impregnation is preferably 110-150°C, and the drying time is preferably 6-24 hours; the calcination temperature is preferably 450-550°C, and the calcination time is preferably 2-8 hours.
[0027] The method for preparing the alumina carrier containing sulfate and phosphate of the present invention comprises the following steps:
[0028] (1) a sodium aluminate solution and an aluminum salt solution containing sulfate are mixed, the pH value of which is controlled to be 8.0-8.8, and the mixture is reacted at 50-80° C. for 0.8-2 hours, and then an alkaline phosphorus compound solution is added to adjust the pH value of the system to 9.0-12, and the mixture is reacted for 0.8-2 hours, and then the mixture is heated to 105-150° C. and aged for 3.5-8 hours, and the obtained solid is washed with water and dried to obtain aluminum hydroxide powder containing sulfate and phosphate.
[0029] (2) Aluminum hydroxide powder containing sulfate and phosphate is kneaded with a peptizing agent, extruded into strips, dried, and calcined at 450-700° C. to obtain aluminum oxide containing sulfate and phosphate.
[0030] (3) Alumina containing sulfate and phosphate is treated with air containing water vapor at 580-700° C. for 2-30 hours, wherein the gas / solid volume ratio is controlled to be 500-1000:1 during the water vapor treatment, and the mass ratio of the water vapor to the alumina containing sulfate and phosphate is 1:80-400.
[0031] In the above method, step (1) is to prepare aluminum hydroxide powder containing sulfate and phosphate. The alkaline phosphorus-containing compound is selected from one or more of sodium phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, sodium hexametaphosphate, sodium triphosphate, sodium tripolyphosphate, sodium pyrophosphate, potassium pyrophosphate, sodium hypophosphite, tetrasodium pyrophosphate, sodium ethylenediaminetetramethylene phosphate, sodium glycerophosphate, sodium dihydrogen pyrophosphate, potassium dihydrogen pyrophosphate, sodium monofluorophosphate and sodium chloride, preferably sodium phosphate or sodium dihydrogen phosphate. The aluminum salt containing sulfate is preferably aluminum sulfate or ammonium aluminum sulfate.
[0032] Step (2) is to shape the aluminum hydroxide powder, wherein the peptizing agent is an acid solution, wherein the acid is selected from one or more of hydrochloric acid, nitric acid, acetic acid and citric acid, and the concentration of the acid contained in the peptizing agent is preferably 2-18% by mass, more preferably 5-18% by mass, and the mass ratio of the peptizing agent to the peptized powder is preferably 0.5-0.9. The drying temperature in step (2) is preferably 100-200°C, and the time is preferably 4-24 hours. The calcination temperature is preferably 500-680°C, and the calcination time is preferably 2-6 hours.
[0033] The method (3) is to treat the formed carrier in step (2) with steam to increase the macropore content. The steam treatment temperature is preferably 600-680°C, the water used for the steam treatment is preferably saturated steam at 50-150°C, the steam treatment time is preferably 20-24 hours, the gas / solid volume ratio controlled during the steam treatment is preferably 600-800:1, and the mass ratio of the steam used for the steam treatment to the alumina containing sulfate and phosphate is preferably 1:80-200.
[0034] The catalyst of the present invention needs to be reduced with hydrogen before use, the reduction temperature is preferably 450-520°C, the reduction time is preferably 2-6 hours, and the reduction gas / agent volume ratio is preferably 500-1500:1.
[0035] The catalyst of the present invention is suitable for the catalytic reforming reaction of hydrocarbons. The reforming reaction conditions are: pressure 0.1-10.0MPa, preferably 0.3-2.5MPa, temperature 370-600°C, preferably 450-550°C, hydrogen / hydrocarbon volume ratio 300-3000, preferably 600-1500, feed mass space velocity 0.1-20.0h -1 , preferably 0.5~5.0h -1 .
[0036] The hydrocarbon raw material is straight-run naphtha with a distillation range of 40 to 230° C., or naphtha blended with coking, catalytic cracking, hydrocracking, coal liquefaction, condensate oil, ethylene cracking raffinate oil and the like in petroleum processing.
[0037] The present invention is further described below by way of examples, but the present invention is not limited thereto.
[0038] In the examples and comparative examples, the specific surface area, pore volume and pore distribution of the carrier are determined by low-temperature N2 adsorption method, the specific surface area is calculated by BET method, the liquid nitrogen adsorption volume at a relative pressure (P / P0) of about 0.98 is taken as the total pore volume of the sample, and the pore size distribution is calculated according to SH / T0572-1993 method.
[0039] Example 1
[0040] The gamma-Al2O3 carrier containing phosphate and sulfate described in the present invention is prepared.
[0041] (1) Preparation of aluminum hydroxide powder containing sulfate and phosphate
[0042] In a 3L stainless steel kettle, add 500mL of 200g / L sodium aluminate solution (with an alumina content of 62% by mass and a Na2O content of 37.5% by mass), add 8mL of 65g / L aluminum sulfate solution, adjust the pH value of the slurry to 8.5, and heat to 60°C. Stir well for neutralization reaction for 60min, then add 10mL of 15g / L sodium phosphate solution, adjust the pH value of the system to 9.0, continue stirring for 60min to react, and then heat to 120°C for aging for 4h.
[0043] The aged slurry was filtered, and the obtained filter cake was washed with 90°C deionized water, with the amount of water used for each wash being 500 mL, for a total of 6 washes. The filter cake obtained from the last wash was dried at 120°C for 6 hours to obtain aluminum hydroxide powder containing sulfate and phosphate, wherein the aluminum oxide content was 70% by mass.
[0044] (2) Preparation of alumina carrier containing sulfate and phosphate
[0045] The aluminum hydroxide powder containing sulfate and phosphate prepared in step (1) is kneaded uniformly according to the mass ratio of powder: sesbania powder: nitric acid: acetic acid: citric acid: water = 50:1:2:2:4:38, and then extruded into strips. The wet strips are dried at 120°C for 12 hours and calcined at 650°C for 4 hours to obtain aluminum oxide containing sulfate and phosphate. Air containing saturated water vapor (saturated steam pressure 0.02 MPa) at 60°C is introduced and steam treated at 650°C for 24 hours. During the treatment, the gas / solid volume ratio of the air containing water vapor to the aluminum oxide is controlled to be 700:1, and the mass ratio of the water vapor to the aluminum oxide containing sulfate and phosphate is 1:150, to obtain a γ-Al2O3 carrier Su-1 containing sulfate and phosphate, wherein SO4 2- The content is 0.85% by mass PO4 3- The content is 1.84% by mass, and the sodium content based on alumina is 0.012% by mass. Its physical properties are shown in Table 1.
[0046] Example 2
[0047] An alumina carrier containing sulfate and phosphate was prepared according to the method of Example 1, except that in step (1), after adding aluminum sulfate solution to the sodium aluminate solution for neutralization reaction, 12 mL of sodium dihydrogen phosphate solution with a concentration of 15 g / L was added to adjust the pH value of the system to 9.0, and stirring was continued for 60 min to react, and then heated to 110° C. for aging for 6 h. The aged slurry was filtered, and the obtained filter cake was washed with deionized water at 90° C., with the amount of water used for each washing being 500 mL, and washed 15 times in total. The filter cake obtained from the last washing was dried at 120° C. for 6 hours to obtain aluminum hydroxide powder containing sulfate and phosphate, wherein the aluminum oxide content was 70% by mass.
[0048] Take the above aluminum hydroxide powder, mix and knead it evenly according to the mass ratio of powder: sesbania powder: nitric acid: acetic acid: citric acid: water = 50:1:2:2:4:38, then extrude it into strips, dry the wet strips at 120°C for 12 hours, and roast them at 650°C for 4 hours to obtain aluminum oxide containing sulfate and phosphate. Pass air containing saturated water vapor (saturated steam pressure 0.1MPa) at 100°C and steam treat it at 550°C for 4 hours. During the treatment, the gas / solid volume ratio of the air containing water vapor to the aluminum oxide is controlled to be 700:1, and the mass ratio of the water vapor used to the aluminum oxide containing sulfate and phosphate is 1:100, to obtain a γ-Al2O3 carrier Su-2 containing sulfate and phosphate, wherein SO4 2- The content is 0.65% by mass PO4 3- The content is 1.29% by mass, and the sodium content based on alumina is 0.010% by mass. Its physical properties are shown in Table 1.
[0049] Comparative Example 1
[0050] The carrier was prepared according to the method of Example 1, except that the alumina containing sulfate and phosphate obtained after calcination in step (2) was used as the carrier, denoted as DBSu-1, and no steam treatment was performed. The physical properties of the carrier are shown in Table 1.
[0051] Comparative Example 2
[0052] The carrier was prepared according to the method of Example 2, except that the alumina containing sulfate and phosphate obtained after calcination in step (2) was used as the carrier, denoted as DBSu-2, and no steam treatment was performed. The physical properties of the carrier are shown in Table 1.
[0053] Comparative Example 3
[0054] Phosphate and sulfate are introduced during the molding process to prepare a γ-Al2O3 carrier containing phosphate and sulfate.
[0055] High-purity pseudo-boehmite powder (produced by Sasol, Germany, brand SB) produced by alkoxyaluminum hydrolysis method was mixed and kneaded uniformly according to the mass ratio of powder: methylcellulose: nitric acid: acetic acid: citric acid: phosphoric acid: ammonium sulfate: water = 50:1:2:2:4:0.6:0.25:40, and then extruded into strips. The wet strips were dried at 120°C for 12 hours and calcined at 650°C for 4 hours to obtain a γ-Al2O3 carrier DBSu-3 containing phosphate and sulfate, wherein SO4 2- The content is 0.65% by mass PO4 3- The content is 1.29% by mass, and the sodium content based on alumina is 0.005% by mass. The physical properties of the carrier are shown in Table 1.
[0056] Comparative Example 4
[0057] Take the carrier DBSu-3 prepared in Comparative Example 3 and treat it with steam according to the method of Example 2 (2) to obtain the γ-Al2O3 carrier DBSu-4 containing sulfate and phosphate. Its physical properties are shown in Table 1.
[0058] Example 3
[0059] Preparation of the catalyst of the present invention.
[0060] Take 50 grams of the carrier Su-1 prepared in Example 1, and prepare an impregnation solution with chloroplatinic acid, ammonium perrhenate, indium chloride and hydrochloric acid so that the impregnation solution contains 0.25% Pt, 0.42% Re, 0.20% In and 1.8% Cl (relative to the mass of alumina), and the liquid / solid volume ratio is 1.5. The carrier and the impregnation liquid were poured into a 500 ml flask, and impregnated on a rotary vacuum evaporator (produced by Shanghai Yarong Biochemical Instrument Factory) at 30°C, 0.008 MPa, and a rotation speed of 0.03 m / s for 3 hours. The solid was dried under reduced pressure at 70°C, dried at 120°C for 12 hours, calcined in dry air at 500°C and a gas / agent volume ratio of 700 for 4 hours, and then reduced with H2 at 480°C and a gas / agent volume ratio of 700 for 4 hours to obtain catalyst Cat-1, whose composition is shown in Table 2, and the spherical aberration corrected scanning transmission electron microscopy (AC-STEM) image is shown in Figure 1 . Figure 1 It shows that the Pt in the catalyst is mostly distributed as single atoms or diatoms, with only a small number of large Pt atomic clusters.
[0061] Example 4
[0062] The catalyst was prepared according to the method of Example 3, except that the carrier used was Su-2, and the prepared impregnation solution contained 0.15% In (relative to the mass of alumina). Catalyst Cat-2 was obtained after drying, calcination and reduction. Its composition is shown in Table 2.
[0063] Example 5
[0064] The catalyst was prepared according to the method of Example 3, except that indium chloride was replaced with yttrium nitrate and the impregnation solution contained 0.30% Y (relative to the mass of alumina). Catalyst Cat-3 was obtained after drying, calcination and reduction. Its composition is shown in Table 2.
[0065] Example 6
[0066] The catalyst was prepared according to the method of Example 3, except that the carrier used was Su-2, indium chloride was replaced by yttrium nitrate when preparing the impregnation solution, and Y was contained in the impregnation solution at 0.30% (relative to the mass of alumina). After drying, calcination and reduction, the catalyst Cat-4 was obtained, and its composition is shown in Table 2.
[0067] Example 7
[0068] The catalyst was prepared according to the method of Example 3, except that the carrier used was Su-2, and the prepared impregnation solution contained Pt0.25%, Re0.42% and Cl1.8% (relative to the mass of alumina). After drying, calcination and reduction, the catalyst Cat-5 was obtained. Its composition is shown in Table 2.
[0069] Comparative Example 5
[0070] The catalyst was prepared according to the method of Example 3, except that the carrier used was DBSu-1, and the catalyst DBCat-1 was obtained. The catalyst DBCat-1 was obtained by drying, calcining and reducing. The composition of the catalyst is shown in Table 2, and the spherical aberration corrected scanning transmission electron microscope (AC-STEM) image is shown in Figure 2 , Figure 2 It shows that Pt in the catalyst exists mostly in large atomic clusters, with less single or diatomic distribution.
[0071] Comparative Example 6
[0072] The catalyst was prepared according to the method of Example 4, except that the carrier used was DBSu-2. After drying, calcination and reduction, the catalyst DBCat-2 was obtained, and its composition is shown in Table 2.
[0073] Comparative Example 7
[0074] The catalyst was prepared according to the method of Example 5, except that the carrier used was DBSu-1. After drying, calcination and reduction, the catalyst DBCat-3 was obtained, and its composition is shown in Table 2.
[0075] Comparative Example 8
[0076] The catalyst was prepared according to the method of Example 4, except that the carrier used was DBSu-3. After drying, calcination and reduction, the catalyst DBCat-4 was obtained, and its composition is shown in Table 2.
[0077] Comparative Example 9
[0078] The catalyst was prepared according to the method of Example 4, except that the carrier used was DBSu-4. After drying, calcination and reduction, the catalyst DBCat-5 was obtained, and its composition is shown in Table 2.
[0079] Comparative Example 10
[0080] The catalyst was prepared according to the method of Example 5, except that the carrier used was DBSu-4. After drying, calcination and reduction, the catalyst DBCat-6 was obtained, and its composition is shown in Table 2.
[0081] Comparative Example 11
[0082] The catalyst was prepared according to the method of Example 7, except that the carrier used was DBSu-2. After drying, calcination and reduction, the catalyst DBCat-7 was obtained, and its composition is shown in Table 2.
[0083] Example 8
[0084] 50 mL of catalyst was loaded on the medium-sized device, and the reaction performance of the catalyst was evaluated using refined naphtha with the properties listed in Table 3 as the raw material. The aromatics potential content of naphtha in Table 3 was 47.1% by mass. The evaluation conditions were: reaction temperature of 520°C, pressure of 0.7 MPa, feed mass space velocity of 1.85 h-1 , the hydrogen / hydrocarbon volume ratio is 1000:1, and the results of each catalyst reacting for 24 hours and 500 hours are shown in Table 4.
[0085] As can be seen from Table 4, compared with the comparative catalyst, the catalyst of the present invention has higher liquid yield, aromatics yield and aromatics conversion rate ((ratio of aromatics yield to aromatics latent content)×100%), indicating that the catalyst of the present invention has higher aromatization activity and selectivity.
[0086] Table 1
[0087]
[0088] Table 2
[0089]
[0090] Table 3
[0091]
[0092] Table 4
[0093]
Claims
1. A naphtha catalytic reforming catalyst, comprising an alumina carrier containing sulfate and phosphate and components having the following contents based on the alumina: The Group VIII metal is selected from platinum, the Group VIIB metal is selected from rhenium, and the halogen is selected from chlorine; The preparation method of the alumina carrier containing sulfate and phosphate comprises the following steps: (1) a sodium aluminate solution and an aluminum salt solution containing sulfate are mixed, the pH value of which is controlled to be 8.0-8.8, and the mixture is reacted at 50-80° C. for 0.8-2 hours, and then an alkaline phosphorus compound solution is added to adjust the pH value of the system to 9.0-12, and the mixture is reacted for 0.8-2 hours, and then the mixture is heated to 105-150° C. and aged for 3.5-8 hours, and the obtained solid is washed with water and dried to obtain aluminum hydroxide powder containing sulfate and phosphate. (2) Aluminum hydroxide powder containing sulfate and phosphate is kneaded with a peptizing agent, extruded into strips, dried, and calcined at 450-700° C. to obtain aluminum oxide containing sulfate and phosphate. (3) Alumina containing sulfate and phosphate is treated with air containing water vapor at 580-700° C. for 2-30 hours, wherein the gas / solid volume ratio is controlled to be 500-1000:1 during the water vapor treatment, and the mass ratio of the water vapor to the alumina containing sulfate and phosphate is 1:80-400.
2. The catalyst according to claim 1, characterized in that The catalyst comprises the following components:
3. The catalyst according to claim 1, characterized in that The aluminum oxide containing sulfate and phosphate is prepared from aluminum hydroxide containing sulfate and phosphate, and the aluminum oxide is gamma-aluminum oxide.
4. The catalyst according to claim 1, characterized in that The alumina carrier containing sulfate and phosphate has the following pore diameter distribution: pores with a diameter of 4 to 6 nm account for 4 to 6% of the total pore volume, pores with a diameter of 6 to 10 nm account for 86 to 90% of the total pore volume, pores with a diameter of 10 to 20 nm account for 5 to 7% of the total pore volume, and pores with a diameter greater than 20 nm account for 1 to 3% of the total pore volume.
5. A catalyst according to any one of claims 1 to 4, characterized in that The catalyst also includes 0.05-3.0 mass % of indium or yttrium.
6. The catalyst according to claim 5, characterized in that The catalyst comprises 0.05-1.0 mass % of indium or yttrium.
7. The catalyst according to claim 1, characterized in that The specific surface area of the alumina carrier containing sulfate and phosphate is 190 to 220 m 2 / g, pore volume is 0.4~0.7mL / g.
8. A method for preparing the catalyst according to claim 1, comprising impregnating an alumina carrier containing sulfate and phosphate with a solution containing a Group VIII metal compound, a Group VIIB metal compound and a halogen as an impregnation liquid, and drying and calcining the impregnated solid.
9. The method according to claim 8, characterized in that The Group VIII metal compound is selected from chloroplatinic acid, tetraammonium dichloroplatinum, ammonium chloroplatinate, platinum trichloride, platinum tetrachloride hydrate, dicarbonyl platinum dichloride, dinitrodiaminoplatinum or sodium tetranitroplatinate; the Group VIIB metal compound is selected from perrhenic acid or ammonium perrhenate; and the halogen is chlorine.
10. The method according to claim 8, characterized in that The impregnation solution also contains indium or yttrium compounds.
11. The method according to claim 10, characterized in that The indium or yttrium compound is indium or yttrium nitrate or chloride.
12. The method according to claim 8, characterized in that The impregnation solution contains hydrochloric acid.
13. The catalyst according to claim 1, characterized in that The alkaline phosphorus-containing compound described in step (1) is one or more selected from the group consisting of sodium phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, sodium hexametaphosphate, sodium triphosphate, sodium tripolyphosphate, sodium pyrophosphate, potassium pyrophosphate, sodium hypophosphite, tetrasodium pyrophosphate, sodium ethylenediaminetetramethylene phosphate, sodium glycerophosphate, sodium dihydrogen pyrophosphate, potassium dihydrogen pyrophosphate, sodium monofluorophosphate and sodium chlorophosphate.
14. The catalyst according to claim 1, characterized in that The aluminum salt containing sulfate group described in step (1) is selected from aluminum sulfate or ammonium aluminum sulfate.
15. The catalyst according to claim 1, characterized in that The peptizing agent in step (2) is an acid solution, wherein the acid is selected from one or more of hydrochloric acid, nitric acid, acetic acid and citric acid.