A method for producing and vulcanizing rubber

By spraying ethanol during the rubber vulcanization process and increasing the temperature, the air discharge problem in the mold cavity is solved, the air accumulation defects in complex cavity and low-hardness rubber products are improved, and the appearance quality of the product is significantly improved.

CN116001157BActive Publication Date: 2024-12-06XIAMEN WAEXIM RUBBER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211705153.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-12-06
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

During the rubber molding vulcanization process, it is easy to cause air in the mold cavity not to be discharged, and the mixing rubber is blocked in or between the mold cavity, resulting in unbalanced material defects and heat conduction, resulting in poor appearance, especially in complex structures and typological conditions. Among products with deep cavity, good fluidity and low hardness.

Method used

During the vulcanization process, ethanol is sprayed on the mold cavity and/or the mixing glue until liquid beads are formed. After the mold is closed, the temperature is raised to carry out the vulcanization reaction to ensure that the vulcanization temperature is higher than the vaporization temperature of ethanol and to discharge it into the mold cavity. air.

Benefits of technology

Effectively solve the problems of gas accumulation and air encapsulation, improve the appearance quality of rubber products with complex structure, deep cavity, excellent fluidity of mixing rubber and low hardness, and reduce the gas accumulation defect rate, especially for three-yuan Application defects of ethylene-propylene rubber and high light-filled rubber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116001157B_ABST
    Figure CN116001157B_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing and vulcanizing rubber, and relates to the technical field of rubber production. The method mainly places a rubber mix to be vulcanized in a mold cavity, sprays ethanol on the mold cavity and / or the rubber mix until liquid beads are formed on the inner surface of the mold cavity, and after the mold is closed, the temperature in the cavity and the temperature of the rubber mix are raised to the vulcanization temperature for vulcanization reaction. Through the production and vulcanization method of the rubber product of the invention, the air in the mold cavity can be completely discharged during the vulcanization process, and air is prevented from being blocked in the mold cavity or between the rubber mixes, and the appearance is prevented from being short of material or being immature due to uneven heat conduction, that is, in the rubber vulcanization process, some problems of gas accumulation defects such as complex structure, deep cavity, excessive fluidity of the rubber mix, and low hardness are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber production, in particular to a rubber production and vulcanization method. Background Art

[0002] Rubber refers to a highly elastic polymer material with reversible deformation. It is elastic at room temperature and can produce large deformation under a small external force. It can return to its original shape after the external force is removed. Rubber is divided into two types: natural rubber and synthetic rubber. Natural rubber is processed from the gum extracted from plants such as rubber trees and rubber grass; synthetic rubber is obtained by polymerization of various monomers.

[0003] Vulcanized rubber refers to vulcanized rubber, which has the characteristics of not becoming sticky and not easy to break. Most rubber products are made of this rubber. It is also called cooked rubber, commonly known as rubber or rubber. It is a general term for rubber after vulcanization. After vulcanization, a three-dimensional structure is formed in the raw rubber, which has high elasticity, heat resistance, tensile strength and insolubility in organic solvents. Most rubber products are vulcanized rubber.

[0004] When rubber is vulcanized by compression molding, the mixed rubber needs to be preformed into various suitable shapes, then placed in the mold cavity, the mold is closed and pressurized, and vulcanization is completed in the mold cavity, so that the raw rubber molecular chains are cross-linked and bonded to form a network structure, so as to achieve the tensile strength and resilience of the rubber product.

[0005] At present, a Chinese patent with publication number CN108690207A discloses a three-step vulcanized rubber processing method, which comprises mixing natural rubber and artificial rubber raw materials in a ratio of 7:3, adding 10-20% by mass of dilute sulfuric acid and performing a three-step vulcanization treatment, and finally waiting for natural cooling to room temperature.

[0006] This rubber vulcanization method increases the molecular weight of the rubber through three-step vulcanization, which is beneficial to the improvement of elasticity. However, during the rubber compression molding process, the air in the mold cavity is often not discharged and is blocked by the rubber mix in the mold cavity or between the rubber mixes, resulting in material shortages or poor appearance due to unbalanced heat conduction, especially for products with complex structures, deep mold cavities, excessive fluidity of the rubber mix, and low hardness. This appearance defect is referred to as air accumulation, air pockets, or air inclusions in the industry. Summary of the invention

[0007] The present invention aims at the above technical problems, overcomes the disadvantages of the prior art, and provides a method for producing and vulcanizing rubber.

[0008] In order to solve the above technical problems, the present invention provides a method for producing and vulcanizing rubber.

[0009] Technical effect: The air in the mold cavity can be completely discharged during the vulcanization process to avoid air blockage in the cavity or between the rubber compounds, thereby preventing material shortage or poor appearance due to unbalanced heat conduction, that is, in the rubber vulcanization process, some air accumulation defects with complex structures, deep cavities, excessive fluidity of the rubber compounds, and low hardness are improved.

[0010] The technical solution further defined in the present invention is:

[0011] A method for vulcanizing rubber, mainly comprising placing a rubber mix to be vulcanized in a mold cavity, spraying ethanol on the mold cavity and / or the rubber mix until liquid beads are formed on the inner surface of the mold cavity, and raising the temperature in the mold cavity and the temperature of the rubber mix to a vulcanization temperature after the mold is closed to carry out a vulcanization reaction;

[0012] The sulfidation temperature is greater than or equal to the vaporization temperature of ethanol.

[0013] Furthermore, the ethanol is 75% ethanol or anhydrous ethanol, and the mixed rubber is one of ethylene propylene rubber, styrene butadiene rubber or chloroprene rubber.

[0014] In the above-mentioned method for vulcanizing rubber, the Mooney viscosity (100°C ML1+4) of the mixed rubber is 5 to 40 N·m.

[0015] The present invention also provides a method for producing a rubber product. During the vulcanization process of the rubber product, the rubber is vulcanized by any of the above-mentioned vulcanization methods, and the rubber is composed of the following weight components:

[0016]

[0017]

[0018] The above-mentioned method for vulcanizing rubber comprises the following steps:

[0019] S1, all materials are mixed in proportion, the rubber base material is put into the internal mixer for plasticization for 1 minute, and then white carbon black, carbon black, filler, filler oil and stearic acid are put into the internal mixer for mixing for 3 minutes;

[0020] S2, when the temperature in the internal mixer is 100℃, the rubber is discharged and rolled into sheets using an open mixer and left to stand for 24h;

[0021] S3, putting the sheet rubber material after standing still into an internal mixer, adding functional additives, sulfur and accelerator for internal mixing, and discharging the rubber when the temperature reaches 85°C, adjusting the roller distance on the open mixer to 1.2mm for thin pass 2 times, adjusting to 5mm for rolling 3 times, and adjusting to 8mm for sheeting for standby use;

[0022] S4, forming the thin-passed sheet rubber into a desired shape and weight, placing it in a mold cavity, spraying anhydrous ethanol on the rubber and / or the cavity surface until liquid beads are formed in the mold cavity, closing the mold and vulcanizing for 200 to 300 seconds under a pressure of 15±1MPa and a temperature of 150 to 165°C to obtain a finished rubber product.

[0023] The above-mentioned method for vulcanizing rubber is used for vulcanization, and the filler is clay, kaolin or light calcium.

[0024] The above-mentioned method for vulcanizing rubber is used for vulcanization, and the filling oil is naphthenic oil, paraffin oil or polar oil.

[0025] The above-mentioned method for vulcanizing rubber is used for vulcanization, and the functional additive is zinc oxide or active zinc oxide.

[0026] The above-mentioned method for vulcanizing a rubber is used for vulcanization, and the accelerator is at least one of accelerator TT, accelerator MTT or accelerator BZ.

[0027] The beneficial effects of the present invention are:

[0028] (1) In the present invention, the method of spraying anhydrous ethanol for vulcanization can effectively solve the problem of gas accumulation or wind trapping during the vulcanization process of rubber products, especially for some products with complex structures, deep cavities, excessive fluidity of the mixed rubber, and low hardness, which cannot be solved by conventional methods. The principle is that after the product is sprayed with anhydrous ethanol and molded in the mold, it evaporates into gas due to its lower boiling point when the mold is closed, which increases the air pressure in the mold cavity and forms a positive pressure to the outside. Through the exhaust action of the machine, a gap is generated in the mold, which wraps the air in the cavity and takes it out of the cavity, thereby solving the problem of gas accumulation;

[0029] (2) In the present invention, the vulcanization was performed by spraying distilled water. It was found that distilled water easily causes EPDM rubber to bubble and is not suitable for degassing EPDM rubber. In addition, the degassing agent containing water sometimes has a high boiling point and cannot evaporate in time and will be wrapped in the rubber to produce bubbles. In the rubber containing a large amount of water-absorbing components (inorganic fillers) in the formula, the water will be absorbed after contacting water, causing bubbles or foaming of the product during the vulcanization process. Therefore, the present invention makes up for the application defects of distilled water in EPDM rubber and high light-colored filled rubber.

[0030] (3) The present invention found that the use of anhydrous ethanol (99% alcohol) has a significant improvement effect on the poor gas accumulation of EPDM rubber, high light color filling and low hardness, and low hardness products, thereby optimizing the quality of the corresponding rubber products;

[0031] (4) In the present invention, by comparing the effects of several volatile substances on rubber degassing, an efficient vulcanization method and rubber production method are confirmed, which improves some gas accumulation defects such as complex structures, deep cavities, excessive fluidity of mixed rubbers, and low hardness, and supplements the application defects of distilled water in EPDM rubber and high light-colored filled rubber, which has great application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the appearance diagram of the SBR pedal skin;

[0033] Figure 2 This is the appearance diagram of the CR low hardness bellows. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, a detailed description is given below in conjunction with the accompanying drawings and specific embodiments. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0036] This embodiment provides a method for producing a rubber product, wherein the rubber product is composed of the following components by weight:

[0037]

[0038] The filler is clay, kaolin or light calcium; the filling oil is cyclohexane oil, paraffin oil or polar oil; the functional additive is zinc oxide or active zinc oxide; and the accelerator is at least one of accelerator TT, accelerator MTT or accelerator BZ.

[0039] When preparing rubber products, the following steps are included:

[0040] S1, all materials are mixed in proportion, the rubber base material is put into the internal mixer for plasticization for 1 minute, and then white carbon black, carbon black, filler, filler oil and stearic acid are put into the internal mixer for mixing for 3 minutes;

[0041] S2, when the temperature in the internal mixer is 100℃, the rubber is discharged and rolled into sheets using an open mixer and left to stand for 24h;

[0042] S3, putting the sheet rubber material after standing still into an internal mixer, adding functional additives, sulfur and accelerator for internal mixing, and discharging the rubber when the temperature reaches 85°C, adjusting the roller distance on the open mixer to 1.2mm for thin pass 2 times, adjusting to 5mm for rolling 3 times, and adjusting to 8mm for sheeting for standby use;

[0043] S4, forming the thin-passed sheet rubber into a desired shape and weight, placing it in a mold cavity, spraying anhydrous ethanol on the rubber and / or the cavity surface until liquid beads are formed in the mold cavity, closing the mold and vulcanizing for 200 to 300 seconds under a pressure of 15±1MPa and a temperature of 150 to 165°C to obtain a finished rubber product.

[0044] Among them, the most critical step is the vulcanization of rubber, and the specific steps are: placing the rubber mix to be vulcanized in the mold cavity, spraying ethanol on the mold cavity and / or the rubber mix until liquid beads are formed on the inner surface of the mold cavity, and after closing the mold, raising the temperature in the cavity and the temperature of the rubber mix to the vulcanization temperature for vulcanization reaction.

[0045] During vulcanization, the vulcanization temperature is greater than or equal to the vaporization temperature of ethanol (78°C). The ethanol used is 75% ethanol or anhydrous ethanol, and the mixed rubber used is one of ethylene propylene rubber, styrene butadiene rubber or chloroprene rubber. In the vulcanization step, the Mooney viscosity (100°C ML1+4) of the mixed rubber is 5 to 40 N·m.

[0046] The present invention also verifies the effect of using the vulcanization method through several embodiments and comparative examples.

[0047] Embodiment 1: the preparation of SBR pedal skin. The shape of SBR pedal skin is as follows Figure 1 shown.

[0048] Proportion: 100 parts of styrene-butadiene rubber, 20 parts of white carbon black, 60 parts of clay, 10 parts of carbon black, 20 parts of naphthenic oil, 5 parts of active zinc oxide, 1 part of stearic acid, 2 parts of sulfur, and 1.5 parts of accelerator CZ.

[0049] Rubber mixing: prepare the materials, first put the styrene-butadiene rubber into the internal mixer and plasticize for 2 minutes, then put in white carbon black, clay, carbon black, cyclohexane oil, activated zinc oxide, stearic acid and cyclohexane oil and mix for 4 minutes, discharge the rubber when the temperature in the internal mixer reaches 120℃, and use an open mixer to roll it into sheets for standby use; after standing for 24 hours, put the rubber into the internal mixer, add sulfur and accelerator for internal mixing, discharge the rubber when the temperature reaches 85℃, adjust the roller distance on the open mixer to 1mm for thinning 2 times, adjust it to 5mm for rolling 3 times, and adjust it to 8mm for sheeting for standby use.

[0050] Molding: pre-form the rubber into the required shape and weight, put it into the mold cavity of the molded product, spray anhydrous ethanol on the rubber or the surface of the cavity (based on the presence of liquid beads before the mold is closed), close the mold, and vulcanize the product at a pressure of 15±1MPa and a temperature of 155-160℃ for 230s to obtain a vulcanized pedal leather product.

[0051] Example 2, preparation of EPDM wiring harness.

[0052] Proportion: 100 parts of EPDM rubber, 10 parts of white carbon black, 40 parts of carbon black, 30 parts of kaolin, 50 parts of paraffin oil, 5 parts of active zinc oxide, 1 part of stearic acid, 1 part of sulfur, 1.5 parts of accelerator BZ, and 0.4 parts of accelerator TT.

[0053] Rubber mixing: prepare the materials, first put the EPDM rubber into the internal mixer and plasticize it for 1 minute, then put in white carbon black, carbon black, kaolin, paraffin oil, active zinc oxide and stearic acid and mix them for 5 minutes, discharge the rubber when the temperature in the internal mixer reaches 130℃, and use an open mixer to roll it into sheets for standby use. After standing for 24 hours, put the rubber into the internal mixer, add sulfur and accelerator for internal mixing, and discharge the rubber when the temperature reaches 85℃. On the open mixer, adjust the roller spacing to 1mm for thinning 2 times, adjust it to 5mm for rolling 3 times, and adjust it to 8mm for sheeting for standby use.

[0054] Molding: Preform the rubber into the required shape and weight, put it into the mold cavity of the molded product, spray anhydrous ethanol on the rubber or the surface of the cavity (based on the presence of liquid beads before the mold is closed), close the mold, and vulcanize the product at a pressure of 15±1MPa and a temperature of 160-165℃ for 250s to obtain a vulcanized wire harness product.

[0055] Example 3, preparation of CR low hardness corrugated pipe.

[0056] Proportion: 100 parts of chloroprene rubber, 8 parts of white carbon black, 30 parts of carbon black, 50 parts of light calcium, 50 parts of polar oil, 1 part of stearic acid, 5 parts of zinc oxide, 0.5 parts of sulfur, and 1 part of accelerator MTT.

[0057] Rubber mixing: prepare the materials, first put the chloroprene rubber into the internal mixer and plasticize for 1 minute, then put in white carbon black, carbon black, light calcium, polar oil and stearic acid and mix for 3 minutes, discharge the rubber when the temperature in the internal mixer reaches 100℃, and use an open mixer to roll it into sheets for standby use. After standing for 24 hours, put the rubber into the internal mixer again, add zinc oxide, sulfur and accelerator for internal mixing, and discharge the rubber when the temperature reaches 85℃. On the open mixer, adjust the roller spacing to 1.2mm for thinning 2 times, adjust to 5mm for rolling 3 times, and adjust to 8mm for sheeting for standby use.

[0058] Molding: Preform the rubber compound into the required shape and weight, put it into the mold cavity of the molded product, spray anhydrous ethanol on the rubber compound or the surface of the cavity (based on the presence of liquid beads before the mold is closed), close the mold, and vulcanize the product at a pressure of 15±1MPa and a temperature of 150-155℃ for 300s to obtain a vulcanized low-hardness corrugated pipe product.

[0059] In the above three embodiments, the present invention sprays tap water, distilled water, 75% alcohol and anhydrous ethanol during the vulcanization process, and the resulting rubber product gas accumulation defect rate is shown in Table 1. The comparative example is a rubber product prepared by direct vulcanization without spraying the medium.

[0060] Table 1 Gas accumulation rate of each embodiment under different spraying media

[0061]

[0062] It can be seen from Table 1 that the gas accumulation defect rate of the three rubber products sprayed with anhydrous ethanol is greatly reduced. Compared with spraying water, the gas accumulation defect rate is reduced by nearly 20 times, and it is greatly optimized compared with not spraying the medium, which illustrates the superiority of spraying ethanol for vulcanization in this scheme.

[0063] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A method for vulcanizing rubber, Features: Placing the rubber mix to be vulcanized in a mold cavity, spraying ethanol on the mold cavity and / or the rubber mix until liquid beads are formed on the inner surface of the mold cavity, and raising the temperature in the mold cavity and the temperature of the rubber mix to the vulcanization temperature to perform a vulcanization reaction after the mold is closed; The sulfidation temperature is greater than or equal to the vaporization temperature of ethanol; The ethanol is 75% ethanol or anhydrous ethanol, and the mixed rubber is one of ethylene propylene rubber, styrene butadiene rubber or chloroprene rubber.

2. A method for vulcanizing rubber according to claim 1, Features: The Mooney viscosity (100°C ML1+4) of the rubber mix is ​​5 to 40 N·m.

3. A method for producing a rubber product, It is characterized in that Vulcanization is carried out by any one of the rubber vulcanization methods as claimed in claims 1 to 2, and the rubber is composed of the following weight components Rubber base 100 parts 5~25 parts of white carbon black Carbon black 8-45 parts Filler 25~65 parts Filler oil 15-55 parts Functional additives 2-8 parts 0.5-1.5 parts of stearic acid Sulfur 0.5-2.5 parts Accelerator 0.5 to 2 parts.

4. A method for producing a rubber product according to claim 3, It is characterized in that The steps include: S1, all materials are mixed in proportion, the rubber base material is put into the internal mixer for plasticization for 1 minute, and then white carbon black, carbon black, filler, filler oil and stearic acid are put into the internal mixer for mixing for 3 minutes; S2, when the temperature in the internal mixer is 100℃, the rubber is discharged and rolled into sheets using an open mixer and left to stand for 24h; S3, putting the sheet rubber material after standing still into an internal mixer, adding functional additives, sulfur and accelerator for internal mixing, and discharging the rubber when the temperature reaches 85°C, adjusting the roller distance on the open mixer to 1.2mm for thin pass 2 times, adjusting to 5mm for rolling 3 times, and adjusting to 8mm for sheeting for standby use; S4, forming the thin-passed sheet rubber into a desired shape and weight, placing it in a mold cavity, spraying anhydrous ethanol on the rubber and / or the cavity surface until liquid beads are formed in the mold cavity, closing the mold and vulcanizing for 200 to 300 seconds under a pressure of 15±1MPa and a temperature of 150 to 165°C to obtain a finished rubber product.

5. A method for producing a rubber product according to claim 4, Features: The filler is clay, kaolin or light calcium.

6. A method for producing a rubber product according to claim 4, Features: The filler oil is naphthenic oil, paraffin oil or polar oil.

7. The method for producing a rubber product according to claim 4, Features: The functional additive is zinc oxide or active zinc oxide.

8. The method for producing a rubber product according to claim 4, Features: The promoter is at least one of promoter TT, promoter MTT or promoter BZ.

Citation Information

Patent Citations

  • Three step vulcanized rubber processing method

    CN108690207A

  • Rubber vulcanization method and rubber production method

    CN109719871A