A sulfur-resistant and water-resistant CO catalyst and its preparation method and application

Through the synergistic action of the multimetal oxide composite catalyst and the nano-scale TiO2 protective layer, the problem of the catalyst's activity reduction in sulfur-containing and high-water environments is solved, and efficient CO oxidation and long-life catalyst performance are achieved.

CN116020459BActive Publication Date: 2024-11-08WUHAN UNIV (ZHAOQING) INST OF RESOURCES & ENVIRONMENTAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211672804.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-11-08
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

The existing catalysts have low oxidation and purification efficiency of carbon monoxide (CO) under sulfur-containing atmosphere, and lack water resistance and stability, making it difficult to maintain high-efficiency activity in high water and high SO2 environments.

Method used

Using a multimetal oxide composite catalyst, the catalyst is improved by combining the nano-scale TiO2 protective layer through the synergistic effect of support such as ZrO2-WO3 and active components such as PdOx, PtOx and RuO2, and the catalyst has a sulfur resistance and water resistance, and is divided into batches. The calcination forms a uniform mesoporous structure to enhance the stability of the catalyst.

Benefits of technology

The activity and service life of the catalyst are significantly improved, and CO can be effectively degraded under conditions of 100 to 150°C. After 100 hours of continuous testing, the CO conversion rate remains above 90%, and the tolerance to SO2 and water is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000006113600000101
    Figure GHA0000006113600000101
  • Figure GHA0000006113600000111
    Figure GHA0000006113600000111
  • Figure GHA0000006113600000112
    Figure GHA0000006113600000112
Patent Text Reader

Abstract

The invention discloses a sulfur-resistant and water-resistant CO catalyst and its preparation method and application. The catalyst comprises a carrier, an active component attached to the carrier and a protective layer; the carrier is ZrO2-WO3 or ZrO2-WO3-R; the active component is PdO x , PtO x and RuO2. Based on the synergistic effect between the components, the catalyst improves the activity of the catalyst while giving the catalyst excellent sulfur resistance and water resistance; the carrier can provide a large number of loading sites for the active components, improve the sulfur resistance of the catalyst, and cooperate with the nano-scale TiO2 protective layer formed on the surface of the catalyst to greatly improve the stability and water resistance of the catalyst. The catalyst is formed by batch calcination, which can increase the specific surface area of ​​the catalyst and form a uniform mesoporous structure. Based on the characteristics of the catalyst, the T99 of catalytic degradation of CO in thermal desorption exhaust gas is 100-150°C, and after continuous testing for 100h in the presence of 100ppm SO2 and 10vol.% H2O, the CO conversion rate can still be maintained above 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a CO oxidation catalyst, in particular to a sulfur-resistant and water-resistant CO catalyst and a preparation method and application thereof, belonging to the technical field of catalysts. Background Art

[0002] The main air pollutants in sintering flue gas are: CO, NO x , SO2, and particulate matter. Therefore, it is urgent to remove carbon monoxide from sintering flue gas. The original concentration of CO emissions in sintering flue gas is 4000-10000 mg / m 3 , containing HCl, HF, NO x 、SO x The catalytic oxidation method has become the most common method of purifying pollutants in industry because of its advantages such as low ignition temperature, great energy saving, high processing efficiency and no harmful by-products. However, since the sintering flue gas still contains 35mg / m 3 SO2, so CO in sintering flue gas will inevitably contain SO2, thus affecting the oxidation activity of CO. Although few people pay attention to the catalytic oxidation purification of CO in a sulfur-containing atmosphere, it is of great significance to the catalytic field, the resource utilization of pollutants and the establishment of a good ecological environment. Summary of the invention

[0003] In view of the problems existing in the prior art, the first object of the present invention is to provide a sulfur-resistant and water-resistant CO catalyst, which, based on the synergistic effect between the various components, imparts the catalyst with excellent sulfur resistance and water resistance while improving the catalyst activity; the carrier of the present invention can not only provide a large number of loading sites for the active components and improve the sulfur resistance of the catalyst, but also accelerate the migration rate of active oxygen on the catalyst surface, thereby improving the catalytic activity, and cooperate with the nano-scale TiO2 protective layer formed on the catalyst surface to further improve the stability and water resistance of the catalyst.

[0004] The second object of the present invention is to provide a method for preparing a sulfur-resistant and water-resistant CO catalyst, which adopts batch calcination to form the catalyst, which can not only increase the specific surface area of ​​the catalyst and form a uniform mesoporous structure, but also ensure the complete loading and stable adsorption of the active components. The formed nanoscale active components have uniform particle size and distribution, and no agglomeration occurs; further, a uniform nanoscale ceramic protective layer is formed on the surface of the catalyst by calcination, and in the process of ensuring the free migration of active oxygen, the poisoning effect of water and sulfide on the active components of the catalyst is effectively avoided, thereby greatly extending the service life of the catalyst.

[0005] The third object of the present invention is to provide an application of a sulfur-resistant and water-resistant CO catalyst for the degradation of CO in thermal desorption exhaust gas. Based on the CO catalyst provided by the present invention, it can ensure the complete degradation of CO in thermal desorption exhaust gas under various environmental conditions. After testing, the catalyst T99 temperature is 100-150°C, and the CO concentration in the raw gas is 4000ppm. The CO concentration in the gas can be as low as 6ppm, and after continuous testing for 100h in the presence of 100ppm SO2 and 10vol.% H2O, the CO conversion rate can still be maintained above 90%.

[0006] To achieve the above technical objectives, the present invention provides a sulfur-resistant and water-resistant CO catalyst, comprising a carrier, an active component attached to the carrier and a protective layer; the carrier is ZrO2-WO3 or ZrO2-WO3-R, wherein R is at least one of MnO2, CuO, CeO2, Fe2O3 and Co3O4; the active component is PdO x , PtO x and RuO2; the mass ratio of the carrier to the active component is: 152-484:1; the protective layer is a TiO2 protective layer.

[0007] The CO catalyst provided by the present invention is a multi-metal oxide composite catalyst. Based on the synergistic effect between the components, the catalyst improves the activity of the catalyst and at the same time gives the catalyst excellent sulfur resistance and water resistance. The carrier of the present invention can not only provide a large number of loading sites for the active components and improve the sulfur resistance of the catalyst, but also accelerate the migration rate of active oxygen on the catalyst surface, thereby improving the catalytic activity, and cooperate with the nano-scale TiO2 protective layer formed on the catalyst surface to further improve the stability and water resistance of the catalyst.

[0008] The ZrO2 in the carrier provided by the present invention is the only oxide with both acidic and alkaline sites, which can not only increase the effective surface area, provide a suitable pore structure, provide loading sites for active components, but also improve the mechanical strength and thermal stability of the catalyst; WO3 is an acidic carrier, which is difficult to react with sulfur oxides to form sulfates, and weakens the effect of SO2 on the catalyst. Further, the carrier can also introduce R groups composed of transition metal oxides. The introduction of CeO2 can make the carrier form more mesopores, which can improve the carrier's alkali metal and alkaline earth metal accommodation capacity, thereby improving the catalyst's alkali resistance; Fe2O3 has good thermal stability, will not undergo corresponding changes at higher temperatures, and can maintain the stability of the basic structure and pores of the catalyst. The introduction of MnO2, CuO and Co3O4 can increase the oxygen transfer rate and accelerate the catalytic reaction rate.

[0009] The active component in the catalyst provided by the present invention is a noble metal oxide, the platinum metal has excellent low-temperature catalytic activity and stability, and RuO2 has excellent resistance to water poisoning, which can effectively extend the service life of the catalyst.

[0010] As a preferred solution, the catalyst further comprises a protective layer, the protective layer is rutile or anatase TiO2, the protective layer accounts for 3-8% of the total mass of the catalyst, and more preferably, the protective layer accounts for 5% of the total mass of the catalyst.

[0011] TiO2 can be used as both a protective layer for the catalyst and a catalyst structural aid. It can stabilize the structure of the catalytic components and improve the stability of the catalyst. It can also improve the catalyst's resistance to water and sintering, and improve the catalyst's resistance to alkali metals, alkaline earth metals, heavy metals, water, chlorine and sulfur. It can weaken the problem of low catalytic activity or carbon deposition caused by limited oxygen transfer and low dispersion, and extend the service life of the catalyst.

[0012] As a preferred solution, the active component of the catalyst is PdO x For CO oxidation, the catalytic activity is ranked as follows: PdO x >PtO x >RuO2, but the water resistance of the active component is the opposite. The present invention utilizes the synergistic effect between the carrier and the protective layer to form a lattice dislocation between Pd and Ti, and the active oxygen can quickly migrate between the two, which not only improves the catalytic activity of Pd, but also strengthens the water resistance of the Pd catalyst.

[0013] As a preferred solution, when the carrier is ZrO2-WO3, the mass fraction of ZrO2 is preferably 40-70%, and the mass fraction of WO3 is preferably 20-40%. More preferably, the mass fraction of ZrO2 is preferably 65%, and the mass fraction of WO3 is preferably 35%.

[0014] As a preferred solution, when the carrier is ZrO2-WO3-R, the mass fraction of WO3 is 15-35%, the mass fraction of ZrO2 is 35-65%, and the balance is R. More preferably, the ZrO2-WO3-R is a ZrO2-WO3-MnO2-CuO-CeO2-Fe2O3-Co3O4 composite.

[0015] As a preferred solution, the carrier consists of the following components in mass percentage: WO3 15-35%, ZrO2 35-60%, MnO2 5-15%, CuO 5-10%, CeO2 4-10%, Fe2O3 5-10% and Co3O4 3-5%.

[0016] The multi-metal oxide catalytic system constructed by the present invention can greatly improve the activity and service life of the catalyst. The reason is the alloying effect of multiple metals, wherein the electronic conditioning between the noble metals weakens the surface adsorption of SO2 on the active material; the strong interaction between the carrier and the active component not only produces abundant oxygen vacancies and enhances the migration rate of oxygen, but also limits the interaction between SO2 and strongly anchored active species, thereby improving the tolerance of the catalyst to SO2, and further obtaining a catalyst with high catalytic efficiency, not easy to deactivate, strong resistance to sintering, water resistance, sulfur resistance and chlorine resistance, thereby achieving complete conversion of CO in sintering flue gas.

[0017] The present invention also provides a method for preparing a sulfur-resistant and water-resistant CO catalyst, comprising: dissolving a carrier raw material including ammonium metatungstate and a soluble zirconium salt, adding citric acid for complexation, and performing a primary calcination to obtain a carrier; fully impregnating the carrier in an active component solution and performing a secondary calcination to obtain a catalyst precursor; and uniformly coating a protective layer slurry on the surface of the catalyst precursor and performing a third calcination to obtain the catalyst precursor.

[0018] The present invention adopts batch calcination to form the catalyst, which can not only increase the specific surface area of ​​the catalyst and form a uniform mesoporous structure, but also ensure the complete loading and stable adsorption of the active components. The formed nanoscale active components have uniform particle size and distribution without agglomeration. Furthermore, a uniform nanoscale ceramic protective layer is formed on the surface of the catalyst by calcination. In the process of ensuring the free migration of active oxygen, the poisoning effects of water and sulfide on the active components of the catalyst are effectively avoided, thereby greatly extending the service life of the catalyst.

[0019] As a preferred solution, the carrier raw material is ammonium metatungstate, a soluble zirconium salt and a soluble R salt; the soluble R salt is at least one of a soluble manganese salt, a soluble copper salt, a soluble cerium salt, a soluble iron salt and a soluble cobalt salt.

[0020] As a preferred embodiment, the soluble zirconium salt is zirconium nitrate, the soluble manganese salt is manganese nitrate, the soluble copper salt is copper nitrate, the soluble cerium salt is cerium nitrate, the soluble iron salt is iron nitrate, and the soluble cobalt salt is cobalt nitrate.

[0021] As a preferred solution, the active component is at least one of a soluble palladium salt, a soluble platinum salt and a soluble ruthenium salt. Further preferably, the soluble palladium salt is palladium nitrate, the soluble platinum salt is platinum nitrate, and the soluble ruthenium salt is ruthenium chloride. During the impregnation process, in order to ensure sufficient impregnation of the active component, the present invention adopts heating impregnation until the water is completely evaporated, and the impregnation temperature is 50-60°C.

[0022] As a preferred solution, the preparation method further comprises: uniformly coating the protective layer slurry on the catalyst surface and then calcining the catalyst three times to obtain the catalyst.

[0023] As a preferred solution, the preparation process of the protective layer slurry is: water, ammonium bicarbonate and titanium dioxide precursor are fully mixed to obtain a colloid, and the colloid powder is obtained by drying and crushing; the colloid powder and silica sol are mixed and stirred at a speed of 1200-1500 rpm for 2-3 hours to obtain; the titanium dioxide precursor is butyl titanate and / or titanium oxysulfate.

[0024] The invention uses ammonium bicarbonate to provide weak alkaline conditions, and the titanium dioxide precursor is hydrolyzed under the weak alkaline conditions to form titanium dioxide colloid, and then the slurry is prepared through the sol action of silica sol.

[0025] As a preferred solution, the mass ratio of the colloid to the silica sol is 92-97:3-8.

[0026] As a preferred solution, the drying conditions are: temperature of 100-140° C. and time of 2-4 hours.

[0027] As a preferred solution, the molar ratio of the metal element to citric acid in the carrier raw material is 1:1.5-3.

[0028] As a preferred solution, the conditions for the primary calcination are: temperature of 450-500° C. and time of 4-4.5 h.

[0029] As a preferred solution, the conditions for the secondary calcination are: temperature of 450-500° C. and time of 4-4.5 hours.

[0030] As a preferred solution, the conditions for the three calcinations are: temperature of 550-650° C. and time of 4-4.5 h.

[0031] The present invention also provides an application of a sulfur-resistant and water-resistant CO catalyst, which is characterized by being used for the degradation of CO in thermal desorption exhaust gas.

[0032] Based on the CO catalyst provided by the present invention, it is possible to ensure complete degradation of CO in thermal desorption exhaust gas under various environmental conditions. After testing, the catalyst T99 temperature is 100-150°C, and when the CO concentration in the raw gas is 4000ppm, the CO concentration in the gas can be as low as 6ppm, and after continuous testing for 100h in the presence of 100ppm SO2 and 10vol.% H2O, the CO conversion rate can still be maintained above 90%.

[0033] As a preferred solution, the conditions for the catalytic oxidation reaction of CO in the thermal desorption exhaust gas are: fixed bed reactor, reaction temperature of 100-120°C, reaction space velocity of 5000-10000h -1 More preferably, the reaction space velocity is 6000 to 8000 h -1 .

[0034] Compared with the prior art, the beneficial technical effects of the present invention are:

[0035] 1) The CO catalyst provided by the present invention is a multi-metal oxide composite catalyst. Based on the synergistic effect between the components, the catalyst improves the activity of the catalyst and at the same time gives the catalyst excellent sulfur resistance and water resistance. The carrier of the present invention can not only provide a large number of loading sites for the active components and improve the sulfur resistance of the catalyst, but also accelerate the migration rate of active oxygen on the catalyst surface, thereby improving the catalytic activity, and cooperate with the nano-scale TiO2 protective layer formed on the catalyst surface to further improve the stability and water resistance of the catalyst.

[0036] 2) In the technical solution provided by the present invention, batch calcination is used to form the catalyst, which can not only increase the specific surface area of ​​the catalyst and form a uniform mesoporous structure, but also ensure the complete loading and stable adsorption of the active components. The nanoscale active components formed have uniform particle size and distribution without agglomeration. Furthermore, a uniform nanoscale ceramic protective layer is formed on the catalyst surface by calcination. While ensuring the free migration of active oxygen, the poisonous effects of water and sulfide on the active components of the catalyst are effectively avoided, thereby greatly extending the service life of the catalyst.

[0037] 3) In the technical solution provided by the present invention, based on the CO catalyst provided by the present invention, it is possible to ensure complete degradation of CO in the thermal desorption exhaust gas under various environmental conditions. After testing, the catalyst T99 temperature is 100-150°C, and when the CO concentration in the raw gas is 4000ppm, the CO concentration in the gas can be as low as 6ppm, and after continuous testing for 100h in the presence of 100ppm SO2 and 10vol.% H2O, the CO conversion rate can still be maintained above 90%. DETAILED DESCRIPTION

[0038] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0039] Example 1

[0040] Weigh zirconium nitrate (113.24g) and ammonium metatungstate (37.19g) in a beaker of 1000mL deionized water, stir at 1500rpm for 30min to form a uniform solution, add citric acid according to metal ion: citric acid = 1:2 (molar ratio), stir to form a uniform mixed solution, transfer to 80℃ water bath, continue stirring until gel, then dry at 80℃ for 36h, grind the obtained sol-gel product and calcine at 500℃ air atmosphere for 4h to obtain a carrier. Immerse the carrier in platinum nitrate solution for impregnation, heat and stir at 50℃ until the water evaporates, place in an oven at 80℃ for overnight, place the obtained powder in a muffle furnace and heat to 500℃ air atmosphere for calcine for 4h at 2℃ / min, and obtain the catalytic component after cooling. Among them, the carrier is a ZrO2-WO3 composite, in which the ZrO2 content is 65%, the WO3 content is 35%, and the active component is PtO2 with a loading amount of 0.2%.

[0041] Ammonium bicarbonate was added to deionized water to obtain weak alkaline conditions, and then butyl titanate was slowly dripped into the resulting solution, and stirred at a speed of 1200 rpm. After the colloid was formed, silica sol was added, and then stirred at a speed of 1200 rpm for 3 hours to obtain TiO2 slurry, in which the amount ratio of deionized water, ammonium bicarbonate, butyl titanate, and silica sol was 50:10:38:2.

[0042] The TiO2 slurry was sprayed on the catalytic component, dried at 120°C and calcined at 600°C in air atmosphere for 4 hours to obtain a catalyst. The TiO2 loading on the catalytic component was 5 wt%.

[0043] Example 2

[0044] Weigh zirconium nitrate (95.82g), ammonium metatungstate (31.88g), and manganese nitrate (43.28g) in a beaker of 1000mL deionized water, stir at 1500rpm for 30min to form a uniform solution, add citric acid according to metal ion: citric acid = 1:2 (molar ratio), stir to form a uniform mixed solution, transfer to 80℃ water bath, continue stirring until gel, then dry at 80℃ for 36h, grind the obtained sol-gel product and calcine at 500℃ air atmosphere for 4h to obtain a carrier. Immerse the carrier in platinum nitrate solution for impregnation, heat and stir at 50℃ until the water evaporates, place in an oven at 80℃ for drying overnight, place the obtained powder in a muffle furnace and heat to 500℃ air atmosphere at 2℃ / min for calcine for 4h, and obtain the catalytic component after cooling. The carrier is a ZrO2-WO3-MnO2 composite, wherein the content of ZrO2 is 55%, the content of WO3 is 30%, the content of MnO2 is 15%, and the loading amount of the active component PtO2 is 0.2%.

[0045] Ammonium bicarbonate was added to deionized water to obtain weak alkaline conditions, and then butyl titanate was slowly dripped into the resulting solution, and stirred at a speed of 1200 rpm. After the colloid was formed, silica sol was added, and then stirred at a speed of 1200 rpm for 3 hours to obtain TiO2 slurry, in which the amount ratio of deionized water, ammonium bicarbonate, butyl titanate, and silica sol was 50:10:38:2.

[0046] The TiO2 slurry was sprayed on the catalytic component, dried at 120°C and calcined at 600°C in air atmosphere for 4 hours to obtain a catalyst. The TiO2 loading on the catalytic component was 5 wt%.

[0047] Example 3

[0048] Weigh zirconium nitrate (87.11g), ammonium metatungstate (26.56g), manganese nitrate (43.28g), and copper nitrate (30.37g) in a beaker containing 1000mL of deionized water, stir at 1500rpm for 30min to form a uniform solution, add citric acid according to the ratio of metal ions to citric acid = 1:2 (molar ratio), stir to form a uniform mixed solution, transfer to an 80℃ water bath, continue stirring until it is in a gel state, and then dry at 80℃ for 36h. Grind the obtained sol-gel product and calcine it at 500℃ in air atmosphere for 4h to obtain a carrier. Immerse the carrier in a platinum nitrate solution for impregnation, heat and stir at 50℃ until the water evaporates, place in an oven at 80℃ for drying overnight, place the obtained powder in a muffle furnace at 2℃ / min and calcine at 500℃ in air atmosphere for 4h, and obtain the catalytic component after cooling. The carrier is a ZrO2-WO3-MnO2-CuO composite, wherein the content of ZrO2 is 50%, the content of WO3 is 25%, the content of MnO2 is 15%, the content of CuO is 10%, and the loading amount of the active component PtO2 is 0.2%.

[0049] Ammonium bicarbonate was added to deionized water to obtain weak alkaline conditions, and then butyl titanate was slowly dripped into the resulting solution, and stirred at a speed of 1200 rpm. After the colloid was formed, silica sol was added, and then stirred at a speed of 1200 rpm for 3 hours to obtain TiO2 slurry, in which the amount ratio of deionized water, ammonium bicarbonate, butyl titanate, and silica sol was 50:10:38:2.

[0050] The TiO2 slurry was sprayed on the catalytic component, dried at 120°C and calcined at 600°C in air atmosphere for 4 hours to obtain a catalyst. The TiO2 loading on the catalytic component was 5 wt%.

[0051] Example 4

[0052] Weigh zirconium nitrate (87.11g), ammonium metatungstate (26.56g), manganese nitrate (28.85g), copper nitrate (15.19g), and cerium nitrate (12.61g) in a beaker containing 1000mL of deionized water, stir at 1500rpm for 30min to form a uniform solution, add citric acid according to the ratio of metal ions to citric acid = 1:2 (molar ratio), stir to form a uniform mixed solution, transfer to an 80℃ water bath, continue stirring until it is gel-like, and then dry at 80℃ for 36h, grind the obtained sol-gel product and calcine at 500℃ in air atmosphere for 4h to obtain a carrier. Immerse the carrier in platinum nitrate solution for impregnation, heat and stir at 50℃ until the water evaporates, place in an oven at 80℃ for drying overnight, place the obtained powder in a muffle furnace and calcine at 500℃ in air atmosphere at 2℃ / min for 4h, and obtain the catalytic component after cooling. The carrier is a ZrO2-WO3-MnO2-CuO-CeO2 composite, in which the ZrO2 content is 50%, the WO3 content is 25%, the MnO2 content is 10%, the CuO content is 5%, the CeO2 content is 10%, and the active component is a PtO2 loading amount of 0.2%.

[0053] Ammonium bicarbonate was added to deionized water to obtain weak alkaline conditions, and then butyl titanate was slowly dripped into the resulting solution, and stirred at a speed of 1200 rpm. After the colloid was formed, silica sol was added, and then stirred at a speed of 1200 rpm for 3 hours to obtain TiO2 slurry, in which the amount ratio of deionized water, ammonium bicarbonate, butyl titanate, and silica sol was 50:10:38:2.

[0054] The TiO2 slurry was sprayed on the catalytic component, dried at 120°C and calcined at 600°C in air atmosphere for 4 hours to obtain a catalyst. The TiO2 loading on the catalytic component was 5 wt%.

[0055] Example 5

[0056] Weigh zirconium nitrate (87.11g), ammonium metatungstate (26.56g), manganese nitrate (28.85g), copper nitrate (15.19g), cerium nitrate (6.31g), and iron nitrate (25.25g) in a beaker containing 1000mL of deionized water, stir at 1500rpm for 30min to form a uniform solution, add citric acid according to the ratio of metal ions to citric acid = 1:2 (molar ratio), stir to form a uniform mixed solution, transfer to an 80℃ water bath, continue stirring until it is gel-like, and then dry at 80℃ for 36h, grind the obtained sol-gel product and calcine it at 500℃ in air atmosphere for 4h to obtain a carrier. Immerse the carrier in platinum nitrate solution for impregnation, heat and stir at 50℃ until the water evaporates, place in an oven at 80℃ for drying overnight, place the obtained powder in a muffle furnace and calcine at 500℃ in air atmosphere at 2℃ / min for 4h, and obtain the catalytic component after cooling. Among them, the carrier is a ZrO2-WO3-MnO2-CuO-CeO2-Fe2O3 complex, in which the ZrO2 content is 50%, the WO3 content is 25%, the MnO2 content is 10%, the CuO content is 5%, the CeO2 content is 5%, the Fe2O3 content is 5%, and the active component is PtO2 with a loading amount of 0.2%.

[0057] Ammonium bicarbonate was added to deionized water to obtain weak alkaline conditions, and then butyl titanate was slowly dripped into the resulting solution, and stirred at a speed of 1200 rpm. After the colloid was formed, silica sol was added, and then stirred at a speed of 1200 rpm for 3 hours to obtain TiO2 slurry, in which the amount ratio (percentage) of deionized water, ammonium bicarbonate, butyl titanate, and silica sol was 50:10:38:2.

[0058] The TiO2 slurry was sprayed on the catalytic component, dried at 120°C and calcined at 600°C in air atmosphere for 4 hours to obtain a catalyst. The TiO2 loading on the catalytic component was 5 wt%.

[0059] Example 6

[0060] Weigh zirconium nitrate (87.11g), ammonium metatungstate (26.56g), manganese nitrate (23.08g), copper nitrate (15.19g), cerium nitrate (5.05g), iron nitrate (25.25g), and cobalt nitrate (5.44g) in a beaker containing 1000mL of deionized water, stir at 1500rpm for 30min to form a uniform solution, add citric acid according to the ratio of metal ions to citric acid = 1:2 (molar ratio), stir to form a uniform mixed solution, transfer to an 80℃ water bath, continue stirring until it is gel-like, and then dry at 80℃ for 36h, grind the obtained sol-gel product and calcine it at 500℃ in air atmosphere for 4h to obtain a carrier. Immerse the carrier in platinum nitrate solution for impregnation, heat and stir at 50℃ until the water evaporates, place in an oven at 80℃ for drying overnight, place the obtained powder in a muffle furnace and calcine at 500℃ in air atmosphere at 2℃ / min for 4h, and obtain the catalytic component after cooling. Among them, the carrier is a ZrO2-WO3-MnO2-CuO-CeO2-Fe2O3-Co3O4 complex, in which the ZrO2 content is 50%, the WO3 content is 25%, the MnO2 content is 8%, the CuO content is 5%, the CeO2 content is 4%, the Fe2O3 content is 5%, the Co3O4 content is 3%, and the active component is PtO2 with a loading amount of 0.2%.

[0061] Ammonium bicarbonate was added to deionized water to obtain weak alkaline conditions, and then butyl titanate was slowly dripped into the resulting solution, and stirred at a speed of 1200 rpm. After the colloid was formed, silica sol was added, and then stirred at a speed of 1200 rpm for 3 hours to obtain TiO2 slurry, in which the amount ratio of deionized water, ammonium bicarbonate, butyl titanate, and silica sol was 50:10:38:2.

[0062] The TiO2 slurry was sprayed on the catalytic component, dried at 120°C and calcined at 600°C in air atmosphere for 4 hours to obtain a catalyst. The TiO2 loading on the catalytic component was 5 wt%.

[0063] Example 7

[0064] Zirconium nitrate (87.11 g), ammonium metatungstate (26.56 g), manganese nitrate (23.08 g), copper nitrate (15.19 g), cerium nitrate (5.05 g), iron nitrate (25.25 g), and cobalt nitrate (5.44 g) were weighed into a beaker containing 1000 mL of deionized water, and stirred at 1500 rpm for 30 min to form a uniform solution. Citric acid was added at a molar ratio of metal ions to citric acid of 1:2, and the mixture was stirred into a uniform mixed solution and then transferred to a 80°C water bath. Stirring was continued until it became a gel, and then dried at 80°C for 36 h. The obtained sol-gel product was ground and calcined at 500°C in air atmosphere for 4 h to obtain a carrier. The carrier is immersed in a mixed solution of palladium nitrate and platinum nitrate, heated and stirred at 50°C until the water evaporates, placed in an oven at 80°C for overnight drying, and the obtained powder is placed in a muffle furnace and calcined at 500°C in an air atmosphere at 2°C / min for 4 hours, and the catalytic component is obtained after cooling. The carrier is a ZrO2-WO3-MnO2-CuO-CeO2-Fe2O3-Co3O4 complex, wherein the ZrO2 content is 50%, the WO3 content is 25%, the MnO2 content is 8%, the CuO content is 5%, the CeO2 content is 4%, the Fe2O3 content is 5%, the Co3O4 content is 3%, and the active component is a PdO loading of 0.2% and a PtO2 loading of 0.2%.

[0065] Ammonium bicarbonate was added to deionized water to obtain weak alkaline conditions, and then butyl titanate was slowly dripped into the resulting solution, and stirred at a speed of 1200 rpm. After the colloid was formed, silica sol was added, and then stirred at a speed of 1200 rpm for 3 hours to obtain TiO2 slurry, in which the amount ratio of deionized water, ammonium bicarbonate, butyl titanate, and silica sol was 50:10:38:2.

[0066] The TiO2 slurry was sprayed on the catalytic component, dried at 120°C and calcined at 600°C in air atmosphere for 4 hours to obtain a catalyst. The TiO2 loading on the catalytic component was 5 wt%.

[0067] Example 8

[0068] Zirconium nitrate (87.11 g), ammonium metatungstate (26.56 g), manganese nitrate (23.08 g), copper nitrate (15.19 g), cerium nitrate (5.05 g), iron nitrate (25.25 g), and cobalt nitrate (5.44 g) were weighed into a beaker containing 1000 mL of deionized water, and stirred at 1500 rpm for 30 min to form a uniform solution. Citric acid was added at a molar ratio of metal ions to citric acid of 1:2, and the mixture was stirred into a uniform mixed solution and then transferred to a 80°C water bath. Stirring was continued until it became a gel, and then dried at 80°C for 36 h. The obtained sol-gel product was ground and calcined at 500°C in air atmosphere for 4 h to obtain a carrier. The carrier is immersed in a mixed solution of palladium nitrate, platinum nitrate and ruthenium chloride, heated and stirred at 50°C until the water evaporates, placed in an oven at 80°C for overnight drying, and the obtained powder is placed in a muffle furnace and calcined at 500°C in an air atmosphere at 2°C / min for 4 hours, and the catalytic component is obtained after cooling. Among them, the carrier is a ZrO2-WO3-MnO2-CuO-CeO2-Fe2O3-Co3O4 complex, wherein the ZrO2 content is 50%, the WO3 content is 25%, the MnO2 content is 8%, the CuO content is 5%, the CeO2 content is 4%, the Fe2O3 content is 5%, the Co3O4 content is 3%, and the active components are 0.2% of PdO loading, 0.2% of PtO2 loading, and 0.1% of RuO2 loading.

[0069] Ammonium bicarbonate was added to deionized water to obtain weak alkaline conditions, and then butyl titanate was slowly dripped into the resulting solution, and stirred at a speed of 1200 rpm. After the colloid was formed, silica sol was added, and then stirred at a speed of 1200 rpm for 3 hours to obtain TiO2 slurry, in which the amount ratio of deionized water, ammonium bicarbonate, butyl titanate, and silica sol was 50:10:38:2.

[0070] The TiO2 slurry was sprayed on the catalytic component, dried at 120°C and calcined at 600°C in air atmosphere for 4 hours to obtain a catalyst with a TiO2 loading of 5wt% on the substrate.

[0071] The present invention also carried out the following tests on the catalyst obtained in the above embodiment:

[0072] (1) Catalytic activity test:

[0073] The catalysts prepared in Examples 1 to 8 were loaded into a stainless steel fixed bed reactor with an inner diameter of 16 mm, and raw gas was introduced into the reactor for catalytic oxidation. The raw gas consisted of waste gas from thermal desorption of organic polluted soil, including: 4000 ppm CO, 10.5% N2, 10.5% O2, and the reaction space velocity was set to 5000 to 10000 h -1, the reaction pressure was normal pressure, the test temperature at the beginning of the reaction was 60°C, and the specific reaction conditions and results are shown in Table 1.

[0074] Table 1 Combustion conditions and results of catalytic sintering of CO in flue gas by catalysts prepared in Examples 1 to 8 and Comparative Example 1

[0075]

[0076]

[0077] Note: 99 It indicates the reaction temperature when the CO conversion rate reaches 90%.

[0078] It can be seen from Table 1 that the catalysts prepared in Examples 1 to 8 can effectively catalyze and oxidize CO, with low catalytic temperature and high efficiency. The concentration of CO at the outlet is as low as 3 ppm, which can basically achieve complete conversion of CO in sintering flue gas, and is efficient, clean, and has significant energy-saving and emission-reduction effects. In addition, the catalysts of Examples 6 to 8 were tested continuously for 100 hours, and the results showed that no carbon deposits were generated on the catalysts, indicating that the catalysts prepared in the present invention have excellent anti-sintering and anti-carbon deposition properties and are not easy to deactivate.

[0079] (2) Anti-poisoning ability test

[0080] 1. Anti-sulfur ability

[0081] The catalysts prepared in Examples 6 to 8 were loaded into a stainless steel fixed bed reactor with an inner diameter of 16 mm to test the catalytic activity of the catalysts. The specific test conditions were: 4000 ppm CO, 100 ppm SO2, 10.5% N2, 10.5% O2, and T 99 Indicates the catalytic activity of the catalyst. Specific test data are shown in Table 3.

[0082] Table 2 Catalytic activity test results of catalysts before and after catalyst sulfidation

[0083] Example <![CDATA[Fresh Activity (T 99 )]]> <![CDATA[Activity after vulcanization (T 99 )]]> Activity difference (℃) 6 135 150 15 7 100 105 5 8 100 100 0

[0084] 2. Water and sulfur resistance

[0085] The catalysts prepared in Examples 6 to 8 were loaded into a stainless steel fixed bed reactor with an inner diameter of 16 mm to test the catalytic activity of the catalysts. The specific test conditions were: 4000 ppm CO, 100 ppm SO2, 10% H2O, 10.5% N2, 10.5% O2, and T 99 Indicates the catalytic activity of the catalyst. Specific test data are shown in Table 3.

[0086] Table 3 Test results of water and sulfur resistance of catalysts

[0087]

[0088]

[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A sulfur-resistant and water-resistant CO catalytic oxidation degradation catalyst, characterized in that: The invention comprises a carrier, an active component loaded on the carrier and a protective layer; the carrier is ZrO2-WO3 or ZrO2-WO3-R, wherein R is at least one of MnO2, CuO, CeO2, Fe2O3 and Co3O4; the active component is PdO x , PtO x and RuO2; the mass ratio of the carrier to the active component is: 152~484:1; the protective layer is a TiO2 protective layer; the protective layer accounts for 3~8% of the total mass of the catalyst; When the carrier is ZrO2-WO3, the mass fraction of ZrO2 is 40-70%, and the mass fraction of WO3 is 20-40%; When the carrier is ZrO2-WO3-R, the mass fraction of WO3 is 15-35%, the mass fraction of ZrO2 is 35-65%, and the remainder is R.

2. The sulfur-resistant and water-resistant CO catalytic oxidation degradation catalyst according to claim 1, characterized in that: The protective layer is rutile or anatase TiO2.

3. The sulfur-resistant and water-resistant CO catalytic oxidation degradation catalyst according to claim 1, characterized in that: The carrier consists of the following components in percentage by mass: WO3 15-35%, ZrO2 35-60%, MnO2 5-15%, CuO 5-10%, CeO2 4-10%, Fe2O3 5-10% and Co3O4 3-5%.

4. The method for preparing a sulfur-resistant and water-resistant CO catalytic oxidation degradation catalyst according to any one of claims 1 to 3, characterized in that: include: After dissolving the carrier raw materials including ammonium metatungstate and soluble zirconium salt, citric acid is added for complexation, and roasting is performed once to obtain the carrier; The carrier is fully impregnated in the active component solution and then calcined twice to obtain a catalyst precursor; a protective layer slurry is evenly coated on the surface of the catalyst precursor and then calcined three times to obtain the catalyst precursor.

5. The method for preparing a sulfur-resistant and water-resistant CO catalytic oxidation degradation catalyst according to claim 4, characterized in that: The preparation process of the protective layer slurry is as follows: water, ammonium bicarbonate and a titanium dioxide precursor are fully mixed to obtain a colloid, which is then dried and crushed to obtain a colloidal powder; the colloidal powder is mixed with silica sol and stirred at a speed of 1200 to 1500 rpm for 2 to 3 hours to obtain the titanium dioxide precursor; the titanium dioxide precursor is butyl titanate and / or titanium oxysulfate.

6. The method for preparing a sulfur-resistant and water-resistant CO catalytic oxidation degradation catalyst according to claim 5, characterized in that: The titanium dioxide precursor is butyl titanate and / or titanyl sulfate; the mass ratio of the colloid to the silica sol is 92-97:3-8.

7. The method for preparing a sulfur-resistant and water-resistant CO catalytic oxidation degradation catalyst according to claim 4, characterized in that: The molar ratio of the metal element to citric acid in the carrier raw material is 1:1.5-3; the conditions for the first calcination are: temperature of 450-500°C, time of 4-4.5h; the conditions for the second calcination are: temperature of 450-500°C, time of 4-4.5h.

8. The method for preparing a sulfur-resistant and water-resistant CO catalytic oxidation degradation catalyst according to claim 4, characterized in that: The conditions for the three calcinations are: temperature of 550-650° C. and time of 4-4.5 h.

9. Use of the CO catalytic oxidation degradation catalyst according to any one of claims 1 to 3 or the catalyst obtained by the preparation method according to any one of claims 4 to 8, characterized in that: Used for oxidative degradation of CO in thermal desorption exhaust gas.