Catalytic cracking catalyst, catalytic cracking aid and preparation method and application thereof
By using copper-containing perovskite as heating material for catalytic cracking reaction, self-heating is achieved through redox reaction, which solves the problems of insufficient heat capacity and poor heating effect in catalytic cracking reaction, provides stable and efficient heating effect, and improves the High-value products yield.
Patent Information
- Application Number
- CN202111258188.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-27
AI Technical Summary
The existing catalytic cracking catalyst has limited heat capacity, making it difficult to increase the reaction temperature, and it will have adverse effects when increasing the agent-oil ratio. The existing heating materials cannot achieve good heating effects while maintaining the product distribution well.
Using copper-containing perovskite as heating material, self-heating is achieved through redox reaction, and a catalytic cracking auxiliary is prepared. The configuration structure of copper-containing perovskite is stable, which is used to provide heat during catalytic cracking reaction and is combined with the catalyst. Use in combination.
This catalytic cracking additive has good heating effect in catalytic cracking reaction, maintains efficient heating for a long time, and has little toxic effect on the catalyst, does not affect the catalytic effect, and improves the yield of high-value products.
Smart Images

Figure CN116020485B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of catalytic cracking, and in particular, to a catalytic cracking catalyst, a catalytic cracking aid, and a preparation method and application thereof. Background Art
[0002] The catalytic cracking unit is the core equipment of the secondary processing of the refinery. It is a process that converts the distillate oil or residual oil obtained from the atmospheric and vacuum tower into fuels such as liquefied gas, gasoline, diesel, or chemical raw materials such as ethylene, propylene, butene, BTX, etc. under the action of catalysts and high temperature. The catalyst is not only the reaction active center of the catalytic cracking reaction, but also the heat and mass transfer carrier of the catalytic cracking regeneration system. The catalyst enters the reactor from the high-temperature regenerator and brings in a large amount of heat, which promotes the occurrence of catalytic cracking reaction. The coke generated by the reaction is loaded on the surface of the catalyst. Then, when entering the regenerator, it burns with oxygen in the air to generate a large amount of heat, completing the transfer and generation of heat.
[0003] With the heavy and inferior processing raw materials, and the requirement for the transformation of oil refining equipment to chemical type, the reaction conditions are more stringent. However, the heat capacity of the catalyst is limited, resulting in limited heat provided to the reaction part, so the reaction temperature is difficult to further increase; at the same time, in order to transfer more heat, the catalyst-oil ratio also increases, which will bring some adverse effects. For this reason, some studies have used heat-generating materials to increase the conversion depth without increasing the catalyst-oil ratio.
[0004] So far, existing heating materials cannot achieve good heating effect while maintaining good product distribution. Summary of the invention
[0005] The purpose of the present disclosure is to provide a catalytic cracking catalyst, a catalytic cracking aid, and a preparation method and application thereof. The catalytic cracking aid has a good heating effect, a small toxic effect on the main agent, and does not affect the catalytic effect when used in a catalytic cracking reaction.
[0006] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a catalytic cracking aid, which comprises, based on the total weight of the catalytic cracking aid, 1-50 weight % of a copper-containing perovskite, 10-40 weight % of a first binder and 20-60 weight % of a first carrier in terms of weight percentage; wherein the content of the copper-containing perovskite is calculated by weight of CuO, and the copper-containing perovskite contains rare earth metal elements and / or alkaline earth metal elements.
[0007] Optionally, the molecular formula of the copper-containing perovskite is ACu x1 B 2 x2 O3;
[0008] Wherein, A includes alkaline earth metal elements and / or rare earth metal elements, B2 One or more selected from titanium, manganese, cobalt, nickel and iron, X1+X2=1, X1 is 0.2-1, preferably 0.2-0.6, X2 is 0-0.8, preferably 0.4-0.8.
[0009] Optionally, based on the weight of copper elements, the low-valent copper on the surface of the catalytic cracking aid accounts for more than 70% of the total weight of copper elements on the surface, and the low-valent copper is +1-valent copper.
[0010] Optionally, the first carrier comprises one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite;
[0011] The first binder includes one or more of aluminum oxide, silicon oxide and aluminum phosphate.
[0012] The second aspect of the present disclosure provides a method for preparing the catalytic cracking aid described in the first aspect of the present disclosure, the method comprising the following steps:
[0013] S1, mixing the copper-containing perovskite, the third binder and the first carrier to obtain a mixed slurry;
[0014] S2, drying and then calcining the mixed slurry;
[0015] Wherein, based on the total dry weight of the mixed slurry, in terms of weight percentage, the mixed slurry includes 1-50 weight % of a copper-containing perovskite, 10-40 weight % of a third binder and 20-60 weight % of a first carrier; wherein the content of the copper-containing perovskite is measured by weight of CuO, the content of the third binder is measured by weight of metal oxide, and the copper-containing perovskite contains rare earth metal elements and / or alkaline earth metal elements;
[0016] Optionally, the calcination conditions in step S2 are: temperature of 500-900° C. and time of 2-20 h.
[0017] Optionally, the method further comprises: before step S1, preparing the copper-containing perovskite by one or more of a co-precipitation method, a sol-gel method and a complexation method.
[0018] Optionally, the third binder includes one or more of aluminum sol, silica sol, phosphate aluminum sol and peptized pseudo-boehmite, and the solid content of the third binder is 20-90% by weight based on metal oxide;
[0019] Optionally, the molecular formula of the copper-containing perovskite is ACu x1 B 2 x2 O3; wherein A includes alkaline earth metal elements and / or rare earth metal elements, B2 One or more selected from titanium, manganese, cobalt, nickel and iron, X1+X2=1, X1 is 0.2-1, preferably 0.2-0.6, X2 is 0-0.8, preferably 0.4-0.8.
[0020] A third aspect of the present disclosure provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises a catalytic cracking main agent and the catalytic cracking auxiliary agent described in the first aspect of the present disclosure.
[0021] Optionally, based on the total weight of the catalytic cracking main agent, the catalytic cracking main agent comprises, in terms of weight percentage, 10-40 weight % of a molecular sieve, 30-60 weight % of a second carrier and 20-40 weight % of a second binder;
[0022] The molecular sieve includes one or more of a FAU structure molecular sieve, an MFI structure molecular sieve and a BEA structure molecular sieve;
[0023] The second carrier comprises one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite;
[0024] The second binder includes one or more of aluminum oxide, silicon oxide and aluminum phosphate.
[0025] Optionally, the weight ratio of the catalytic cracking aid to the catalytic cracking main agent is 1:(1-40).
[0026] Optionally, based on the total weight of the catalytic cracking catalyst, the content of the catalytic cracking aid is 1-20% by weight in terms of weight percentage.
[0027] A fourth aspect of the present disclosure provides a method for catalytic cracking reaction, the method comprising:
[0028] Contacting the crude oil with the catalytic cracking catalyst described in the third aspect of the present disclosure in a catalytic cracking reactor to carry out a catalytic cracking reaction;
[0029] The temperature of the catalytic cracking reaction is 450-650°C, and the catalyst-oil ratio is 5-20.
[0030] Optionally, the method further comprises: before the feedstock oil is brought into contact with the catalytic cracking catalyst, performing reduction pretreatment on the catalytic cracking catalyst or the catalytic cracking aid;
[0031] The reduction pretreatment comprises: contacting the catalytic cracking catalyst or the catalytic cracking aid with a reducing gas, the time of the reduction pretreatment is 0.5-5 minutes, the temperature of the reduction pretreatment is 650-750° C.; the reducing gas comprises one or more of hydrogen, ethylene and methane.
[0032] Optionally, the method further comprises a regeneration process of the catalytic cracking catalyst, wherein the regeneration process comprises the following steps:
[0033] a. Separating the mixed oil obtained from the catalytic cracking reaction to obtain reaction oil gas and spent catalytic material containing spent catalyst and reduced catalytic cracking aid;
[0034] b. allowing the catalytic material to be regenerated to enter a regenerator for regeneration treatment to obtain a regenerated catalytic material comprising a regenerated catalyst and an oxidized catalytic cracking aid;
[0035] c. returning the regenerated catalytic material to the catalytic cracking reactor for continued use or returning the regenerated catalytic material to the catalytic cracking reactor for continued use after reduction pretreatment.
[0036] Optionally, based on the weight of copper element, the low-valent copper on the surface of the catalytic cracking aid that has undergone the reduction pretreatment accounts for more than 70% of the total weight of copper element, and the low-valent copper is +1-valent copper.
[0037] Through the above technical scheme, the present invention uses copper-containing perovskite as a heat-generating material to prepare a self-heating catalytic cracking aid. When the catalytic cracking aid is used in a catalytic cracking reaction, the self-heating of the aid is achieved through the oxidation-reduction reaction of the copper element. The configuration structure of the copper-containing perovskite in the catalytic cracking aid is stable, and it is not easy to lose in the catalytic cracking reaction, which is conducive to maintaining a good heat-generating effect for a long time. In addition, the catalytic cracking aid disclosed in the present invention has a large calorific value and a small toxic effect on the catalytic cracking main agent. When applied to a catalytic cracking reaction, it does not affect the catalytic effect of the catalytic cracking reaction catalyst.
[0038] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0040] Figure 1 It is a copper-containing perovskite LaCu in one embodiment of the present application. x Mn 1-x XRD diffraction pattern of O3. DETAILED DESCRIPTION
[0041] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0042] A first aspect of the present disclosure provides a catalytic cracking aid, which comprises, based on the total weight of the catalytic cracking aid, 1-50 wt % of a copper-containing perovskite, 10-40 wt % of a first binder and 20-60 wt % of a first carrier in terms of weight percentage; wherein the content of the copper-containing perovskite is calculated based on the weight of CuO, and the copper-containing perovskite contains rare earth metal elements and / or alkaline earth metal elements.
[0043] The catalytic cracking aid disclosed in the present invention uses copper-containing perovskite as a heating material and self-heats through a cycle of redox reaction to provide heat for the catalytic cracking reaction. The copper-containing perovskite has a stable structure and is not easy to lose, which is conducive to maintaining a good heating effect for a long time.
[0044] In the present disclosure, the molecular formula of copper-containing perovskite is ACu x1 B 2 x2 O3; wherein A includes alkaline earth metal elements and / or rare earth metal elements, B 2 One or more selected from titanium, manganese, cobalt, nickel and iron, X1+X2=1, X1 is 0.2-1, preferably 0.2-0.6, X2 is 0-0.8, preferably 0.4-0.8.
[0045] In one embodiment of the present disclosure, the low-valent copper on the surface of the catalytic cracking aid accounts for more than 70% of the total weight of the surface copper element, measured by the weight of the copper element, and the low-valent copper is +1-valent copper. When the catalytic cracking aid meeting the above low-valent copper content is used in a catalytic cracking reaction, the product distribution is good and the yield of high-value products is high. The above content is tested by XPS.
[0046] The second aspect of the present disclosure provides a method for preparing the catalytic cracking aid described in the first aspect of the present disclosure, the method comprising the following steps:
[0047] S1, mixing the copper-containing perovskite, the third binder and the first carrier to obtain a mixed slurry;
[0048] S2, drying and then calcining the mixed slurry;
[0049] Wherein, based on the total weight of the mixed slurry, the mixed slurry includes, in terms of weight percentage, 1-50 weight % of copper-containing perovskite, 10-40 weight % of a third binder and 20-60 weight % of a first carrier; wherein the content of the copper-containing perovskite is measured by the weight of CuO, the content of the third binder is measured by the weight of the metal oxide, and the copper-containing perovskite contains rare earth metal elements and / or alkaline earth metal elements.
[0050] In the present disclosure, the mixing method of the copper-containing perovskite, the third binder and the first carrier is conventional in the art, for example, the third binder is first mixed with the first carrier, and then the copper-containing perovskite is added thereto.
[0051] In one embodiment of the present disclosure, the third binder includes one or more of aluminum sol, silica sol, phosphate aluminum sol and peptized pseudo-boehmite, and the solid content of the third binder is 20-90% by weight, for example, 20-40% by weight, calculated as metal oxide.
[0052] In one embodiment of the present disclosure, the calcination conditions are: temperature of 500-900°C, time of 2-20h; preferably, time of 8-15h, temperature of 750-850°C.
[0053] In one embodiment of the present disclosure, the method further comprises: before step S1, preparing the copper-containing perovskite by one or more of coprecipitation, sol-gel and complexation methods, which are conventional in the art.
[0054] For example, copper-containing perovskite LaCu x Mn 1-x The preparation method of O3 comprises the following steps:
[0055] (1) dissolving a copper source, a lanthanum source and a manganese source in deionized water at a stirring speed of 400-700 rpm;
[0056] (2) adding citric acid monohydrate thereto, maintaining the same rotation speed, stirring at 35-55° C. for 30-60 min, and adding ethylene glycol to obtain a mixture;
[0057] (3) heating the mixture obtained in step (1) to 80-100° C., stirring until it reaches a sol state, standing for 70-100 hours, and drying at 90-120° C. overnight;
[0058] (4) heat treating the solid obtained in step (3) at 400-500° C. for 3-6 hours;
[0059] (5) calcining the material obtained in step (4) at 750-1000° C. for 10-15 h to obtain the copper-containing perovskite LaCu x Mn 1-x O3.
[0060] In the present disclosure, the method for preparing a catalytic cracking reaction aid further comprises treating the catalytic cracking reaction aid pre-product obtained after roasting with an ammonium sulfate solution, wherein the ratio of ammonium sulfate, the catalytic cracking reaction aid pre-product on a dry basis and water is (0.3-0.7):1:(8-12), and then rinsing with deionized water, filtering, drying and secondary roasting to obtain the catalytic cracking reaction aid. The secondary roasting temperature is 800-1000°C and the time is 8-12h.
[0061] A third aspect of the present disclosure provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises a catalytic cracking aid and the catalytic cracking aid described in the first aspect of the present disclosure.
[0062] In one embodiment of the present disclosure, based on the total weight of the catalytic cracking main agent, the catalytic cracking main agent includes 10-40 wt% of molecular sieve, 30-60 wt% of the second carrier and 20-40 wt% of the second binder in terms of weight percentage.
[0063] In one embodiment of the present disclosure, the molecular sieve includes one or more of a FAU structure molecular sieve, an MFI structure molecular sieve and a BEA structure molecular sieve. For example, it can be one or more of a Y molecular sieve, a ZSM-5 molecular sieve, and a β molecular sieve. Further, the Y molecular sieve includes one or more of HY, REY, REHY, USY, and a Y molecular sieve containing phosphorus elements and rare earth elements. The ZSM-5 molecular sieve includes one or more of HZSM-5, a ZSM-5 molecular sieve containing phosphorus elements and transition metal elements, and a ZRP molecular sieve, and the transition metal may include one or more of Fe elements, Co elements, Ni elements, Mn elements, Ti elements, Zn elements, Cu elements, Ga elements, and Re elements.
[0064] In one embodiment of the present disclosure, the weight ratio of the catalytic cracking aid to the catalytic cracking main agent is 1:(1-40), preferably 1:(1-25).
[0065] In one embodiment of the present disclosure, based on the total weight of the catalytic cracking catalyst, the content of the catalytic cracking aid is 1-20% by weight in terms of weight percentage.
[0066] In the present disclosure, the rare earth metal element and the alkaline earth metal element include one or more of calcium element, strontium element, barium element and lanthanum element.
[0067] In the present disclosure, the first binder and the second binder are the same or different, and independently include one or more of aluminum oxide, silicon oxide and aluminum phosphate.
[0068] In the present disclosure, the first carrier and the second carrier are the same or different, and independently include one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite.
[0069] In the present disclosure, the average particle size of the catalytic cracking main agent is 70-90 μm.
[0070] A fourth aspect of the present disclosure provides a method for catalytic cracking reaction, the method comprising:
[0071] Contacting the crude oil with the catalytic cracking catalyst described in the third aspect of the present disclosure in a catalytic cracking reactor to carry out a catalytic cracking reaction;
[0072] The temperature of the catalytic cracking reaction is 450-650°C, and the catalyst-oil ratio is 5-20. Preferably, the temperature is 500-600°C, and the catalyst-oil ratio is 5-15.
[0073] In the present disclosure, the catalytic cracking catalyst is reduced by the dry gas produced by the catalytic cracking reaction after entering the reactor. The dry gas includes reducing gases such as hydrogen and ethylene. At this time, the copper element therein is converted into a reduced state under the action of the reducing gas.
[0074] In the present disclosure, the catalyst-oil ratio refers to the mass ratio of the catalytic cracking catalyst to the feedstock oil.
[0075] In one embodiment of the present disclosure, the type of feedstock oil used in the catalytic cracking reaction is conventional in the art and is not specifically required. The feedstock oil may include, for example, hydrotreated oil and / or Wu-mixed oil, wherein the parameters of the Wu-mixed oil are listed in the examples.
[0076] In one embodiment of the present disclosure, the method further includes: before the feedstock oil is contacted with the catalytic cracking catalyst, the catalytic cracking catalyst or the catalytic cracking aid is subjected to reduction pretreatment; the reduction pretreatment includes: contacting the catalytic cracking catalyst or the catalytic cracking aid with a reducing gas, the time of the reduction pretreatment is 0.5-5min, and the temperature of the reduction pretreatment is 650-750°C; the reducing gas includes one or more of hydrogen, ethylene and methane. Further, in terms of the weight of copper element, the low-valent copper on the surface of the catalytic cracking aid that has been subjected to reduction pretreatment accounts for more than 70% of the total weight of the surface copper element, and the low-valent copper is 1-valent copper. The above content is tested by XPS. When the catalytic cracking aid that has been subjected to reduction pretreatment is applied to the catalytic cracking reaction, it is beneficial to optimize the product distribution and further improve the yield of high-value products.
[0077] In one embodiment of the present disclosure, the method further comprises a regeneration process of the catalytic cracking catalyst, wherein the regeneration process comprises the following steps:
[0078] a. Separating the mixed oil obtained from the catalytic cracking reaction to obtain reaction oil gas and spent catalytic material containing spent catalyst and reduced catalytic cracking aid;
[0079] b. allowing the catalytic material to be regenerated to enter a regenerator for regeneration treatment to obtain a regenerated catalytic material comprising a regenerated catalyst and an oxidized catalytic cracking aid;
[0080] c. returning the regenerated catalytic material to the catalytic cracking reactor for continued use or returning the regenerated catalytic material to the catalytic cracking reactor for continued use after reduction pretreatment;
[0081] The temperature of the regeneration treatment is 650-750°C, preferably 670-730°C.
[0082] In the present disclosure, the regeneration method may be, for example, introducing oxygen into the regenerator to oxidize the copper element in the catalytic material to be regenerated.
[0083] In the present disclosure, the content of each component is calculated based on the amount at the time of charging.
[0084] The present invention will be further described below by way of examples, but the present invention is not limited thereto. The instruments and reagents used in the examples and comparative examples of the present invention are commonly used by those skilled in the art unless otherwise specified.
[0085] The FAU structure molecular sieve used in the examples and comparative examples is DASY2.0, and the catalytic cracking main agent is COKC-1, both of which are products of Sinopec Catalyst Company.
[0086] Examples 1-5
[0087] First, prepare copper-containing perovskite. 0.4 Mn 0.6 O3 is used as an example to illustrate the method of preparing copper-containing perovskite.
[0088] (1) 3.94 g (0.016 mol) of copper nitrate trihydrate, 17.65 g (0.041 mol) of lanthanum nitrate hexahydrate, and 8.75 g (0.024 mol) of 50% manganese nitrate were dissolved in 664 g of deionized water at 40° C. under stirring at a speed of 500 rpm;
[0089] (2) adding 34.3 g (0.163 mol) of citric acid monohydrate, maintaining the rotation speed at 500 rpm and the temperature at 40°C, stirring for 30 min, and then adding 10.11 g (0.163 mol) of ethylene glycol;
[0090] (3) heating the mixture obtained in step (2) to 80° C., stirring continuously until a sol is formed, standing for 72 hours, and then drying at 100° C. overnight;
[0091] (4) heat treating the solid obtained in step (3) at 450° C. in a muffle furnace for 3 h;
[0092] (5) The material obtained in step (4) was calcined at 800° C. for 12 h to obtain the copper-containing perovskite LaCu 0.4 Mn 0.6 O3.
[0093] On a dry basis, weigh each component according to the ratio shown in Table 1.
[0094] The first carrier kaolin was prepared into a slurry with a solid content of 30 wt% by using decationized water, and stirred evenly. The pH of the slurry was adjusted to 2.5 with hydrochloric acid, and the pH value was maintained. After standing and aging at 50°C for 1 hour, a binder aluminum sol (alumina content of 21.5 wt%) was added, and stirred for 1 hour to form a colloid. The copper-containing perovskite LaCu 0.4 Mn 0.6 O3, forming a mixed slurry.
[0095] After continued stirring, the mixed slurry was spray dried to prepare a microsphere catalytic cracking aid precursor. The microsphere catalytic cracking aid precursor was then calcined at 500°C for 1 hour to obtain a catalytic cracking aid pre-product. It was then washed with an ammonium sulfate solution at 60°C (the mass ratio of ammonium sulfate, catalytic cracking aid pre-product on a dry basis and water was 0.5:1:10) until the sodium oxide content was less than 0.25% by weight. After that, it was rinsed with deionized water and filtered, dried, and calcined at 850°C for 10 hours to obtain catalytic cracking aids Z-22 to Z-26. XPS was used to test the proportion of low-valent copper on the surface of catalytic cracking aids Z-22 to Z-26 to the total weight of copper elements on the surface area, and the results are listed in Table 2.
[0096] Example 6
[0097] On a dry basis, the catalytic cracking aid Z-27 was prepared according to the ratio shown in Table 1 and the method described in Example 4, except that the copper-containing perovskite used was LaCu 0.2 Mn 0.8 O3 and XPS were used to test the ratio of low-valent copper on the surface of catalytic cracking aid Z-27 to the total weight of copper elements on the surface area. The results are listed in Table 2.
[0098] Example 7
[0099] Before entering the reactor, the catalytic cracking aid Z-25 prepared in Example 4 was subjected to reduction pretreatment using 20% hydrogen (the rest being nitrogen) as a reducing gas, and the pre-reduction treatment was performed at 650° C. for 2 minutes to obtain the catalytic cracking aid Z-25-1. XPS was used to test the ratio of low-valent copper on the surface of the catalytic cracking aid to the total weight of copper elements on the surface area, and the results are listed in Table 2.
[0100] Figure 1 The copper-containing perovskite LaCu prepared for this application X Mn 1-X The XRD diffraction pattern of O3, X is 0.2, 0.4, and 0.6 respectively. There are obvious diffraction peaks at diffraction angles of 23°, 33°, 47°, and 58° in the XRD spectrum, proving that the copper-containing perovskite has an ABO3 configuration.
[0101] The XRD diffraction instrument model is D5005 X-ray diffractometer from Siemens, Germany, and the experimental conditions are Cu target, Kα radiation, solid detector, tube voltage 40 kV, tube current 40 mA, step scan, step size 0.02, preset time 2 s, and scanning range 5-70.
[0102] The instrument model for testing the proportion of low-priced copper is ESCALab250 X-ray photoelectron spectrometer.
[0103] Embodiment 8-14
[0104] Catalytic cracking aids Z-22 to Z-27, Z-25-1 and catalytic cracking main agent were mixed at a weight ratio of 1:19, and aged at 800°C for 12 hours with 100% steam to obtain catalytic cracking catalysts A-22 to A-27, A-25-1. The catalytic cracking main agent is a fresh industrial agent. Based on the total weight of the catalytic cracking main agent, the catalytic cracking main agent contains 28% by weight of alumina, 40% by weight of kaolin and 32% by weight of FAU structure molecular sieve. The properties of the catalytic cracking main agent are listed in Table 3.
[0105] Table 3
[0106]
[0107]
[0108] Comparative Example 1
[0109] On a dry basis, the catalytic cracking aid Z-21 was prepared according to the ratio shown in Table 1 and the method of Example 1. XPS was used to test the ratio of low-valent copper on the surface of the catalytic cracking aid Z-21 to the total weight of copper elements on the surface area, and the results are listed in Table 2.
[0110] Table 1
[0111]
[0112] Comparative Example 2
[0113] The catalytic cracking aid Z-21 prepared in Comparative Example 1 was used as the catalytic cracking aid, and the method of Example 8 was used to prepare the catalytic cracking catalyst A-21.
[0114] Comparative Example 3
[0115] Catalytic cracking catalyst D was prepared by the method of Example 1, except that the copper-containing perovskite and the molecular sieve were in the same particle, and based on the total weight of the catalytic cracking catalyst, the catalytic cracking catalyst contained 1 wt% of copper-containing perovskite, 30.4 wt% of FAU structure molecular sieve, 27.6 wt% of alumina and 41 wt% of kaolin in terms of weight ratio. XPS was used to test the ratio of low-valent copper on the surface of the catalytic cracking catalyst D to the total weight of copper elements on the surface area, and the results are listed in Table 2.
[0116] Test Example 1
[0117] The catalytic cracking catalysts A-22 to A-27, A-25-1, A-21, and D prepared above were subjected to the ACE evaluation of the feedstock oil. The properties of the evaluated feedstock oil are shown in Table 4 below.
[0118] Table 4
[0119]
[0120] The catalytic cracking catalysts prepared in Examples 8-14 and Comparative Examples 2-3 were fed into a catalytic cracking fixed fluidized bed micro-ACE reactor for catalytic cracking reaction. The reaction starting temperature was set at 530°C, the catalyst-oil ratio was 5, the measurement point of the bed temperature after the reaction was in the middle of the bed of the reactor, and the reaction ended 70s after the feed oil was introduced. The reaction temperature control point was in the middle of the reactor. The reaction temperature changes were recorded and listed in Table 2.
[0121] Table 2
[0122] Catalyst No. A-22 A-23 A-24 A-25 A-26 A-27 A-25-1 A-21 D Additive No. Z-22 Z-23 Z-24 Z-25 Z-26 Z-27 Z-25-1 Z-21 - Reaction starting temperature / ℃ 530 530 530 530 530 530 530 530 530 Bed temperature after reaction / ℃ 531.3 531.8 533.1 534.7 534.4 534.3 530.5 522.7 531.5 Temperature change / ℃ 1.3 1.8 3.1 4.7 4.4 4.3 0.5 -7.3 1.5 Low-price copper ratio / % 14 12 11.7 9.3 7.2 9.8 95 - 13.5
[0123] Since the heat generated during the reduction of copper elements is not included in Table 2, the temperature change value of the reduced additive Z-25-1 is small. In actual production, the heat generated by this part of the reduction can be used.
[0124] The low-valent copper ratio in Table 2 refers to the ratio of +1-valent copper on the surface of the catalytic cracking aid to the total amount of copper elements on the surface.
[0125] According to the data in Table 2, when the catalytic cracking aid using the copper-containing perovskite of the present application as a heat-generating material is used in a catalytic cracking reaction, the heat-generating effect is significant compared with the catalytic cracking aid without the copper-containing perovskite.
[0126] Test Example 2
[0127] The distribution of catalytic cracking products of catalytic cracking catalysts A-21, A-25, A-25-1 and D was analyzed by online composition analysis using Agilent 6890GC (TCD detector); the liquid products were collected and weighed offline, and simulated distillation analysis and PONA analysis were performed; the ACE device was equipped with a CO2 converter and an online CO2 infrared detector for online analysis of the total amount of coke generated; the mass of all products was normalized and the material balance was calculated, and the results are listed in Table 5. The conversion rate refers to the conversion rate calculated for products other than slurry oil and diesel.
[0128] Table 5
[0129]
[0130]
[0131] According to the data in Tables 2 and 5, the catalytic cracking catalyst A-21 without copper-containing perovskite has a high yield of high-value products such as liquefied gas and gasoline, but its heating effect is not good; the catalyst A-25-1 that has undergone reduction pretreatment has a better product distribution than the catalyst A-25 that has not undergone reduction pretreatment, and the yield of high-value products such as liquefied gas and gasoline is higher. In addition, according to the data of catalyst D, when the copper-containing perovskite and molecular sieve are in different particles, their catalytic performance on the main agent is less affected, the coke is lower, and the yield of high-value products such as liquefied gas and gasoline is higher. Therefore, distributing the copper-containing perovskite and molecular sieve in different particles and performing reduction pretreatment before the catalytic cracking reaction can achieve the effect of optimizing the product distribution while obtaining a higher calorific value.
[0132] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0133] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0134] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A catalytic cracking aid, characterized in that: Based on the total weight of the catalytic cracking aid, the catalytic cracking aid comprises, in terms of weight percentage, 1-50 weight % of a copper-containing perovskite, 10-40 weight % of a first binder and 20-60 weight % of a first carrier; wherein the content of the copper-containing perovskite is based on the weight of CuO, and the copper-containing perovskite contains rare earth metal elements and / or alkaline earth metal elements; The molecular formula of the copper-containing perovskite is ACu x1 B 2 x2 O3; Wherein, A includes alkaline earth metal elements and / or rare earth metal elements, B 2 One or more selected from titanium, manganese, cobalt, nickel and iron, X1+X2=1, X1 is 0.2-1, X2 is 0-0.8; Calculated by the weight of copper elements, the low-valent copper on the surface of the catalytic cracking aid accounts for more than 70% of the total weight of the surface copper elements, and the low-valent copper is +1-valent copper.
2. The catalytic cracking aid according to claim 1, wherein X1 is 0.2-0.
6.
3. The catalytic cracking aid according to claim 1, wherein X2 is 0.4-0.
8.
4. The catalytic cracking aid according to claim 1, wherein The first carrier comprises one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite; The first binder includes one or more of aluminum oxide, silicon oxide and aluminum phosphate.
5. A method for preparing the catalytic cracking aid according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: S1, mixing the copper-containing perovskite, the third binder and the first carrier to obtain a mixed slurry; S2, drying and then calcining the mixed slurry; Wherein, based on the total dry weight of the mixed slurry, in terms of weight percentage, the mixed slurry includes 1-50 weight % of a copper-containing perovskite, 10-40 weight % of a third binder and 20-60 weight % of a first carrier; wherein the content of the copper-containing perovskite is measured by weight of CuO, the content of the third binder is measured by weight of metal oxide, and the copper-containing perovskite contains rare earth metal elements and / or alkaline earth metal elements; The molecular formula of the copper-containing perovskite is ACu x1 B 2 x2 O3; wherein A is selected from alkaline earth metal elements and / or rare earth metal elements, B 2 One or more selected from titanium, manganese, cobalt, nickel and iron, X1+X2=1, X1 is 0.2-1, and X2 is 0-0.
8.
6. The method according to claim 5, wherein: The calcination conditions in step S2 are: temperature of 500-900° C. and time of 2-20 h.
7. The method according to claim 5, wherein: The method further includes: before step S1, preparing the copper-containing perovskite by one or more of a coprecipitation method, a sol-gel method and a complex method.
8. The method according to claim 5, wherein: The third binder includes one or more of aluminum sol, silica sol, phosphate aluminum sol and peptized pseudo-boehmite. The solid content of the third binder is 20-90% by weight based on metal oxide.
9. The method according to claim 5, wherein: X1 is 0.2-0.
6.
10. The method according to claim 5, wherein: X2 is 0.4-0.
8.
11. A catalytic cracking catalyst, characterized in that: The catalytic cracking catalyst comprises a catalytic cracking main agent and a catalytic cracking aid as claimed in any one of claims 1 to 4.
12. The catalytic cracking catalyst according to claim 11, wherein Based on the total weight of the catalytic cracking main agent, the catalytic cracking main agent comprises 10-40 weight percent of a molecular sieve, 30-60 weight percent of a second carrier and 20-40 weight percent of a second binder in terms of weight percentage; The molecular sieve includes one or more of a FAU structure molecular sieve, an MFI structure molecular sieve and a BEA structure molecular sieve; The second carrier comprises one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite; The second binder includes one or more of aluminum oxide, silicon oxide and aluminum phosphate.
13. The catalytic cracking catalyst according to claim 11, wherein The weight ratio of the catalytic cracking aid to the catalytic cracking main agent is 1:(1-40).
14. The catalytic cracking catalyst according to claim 11, wherein Based on the total weight of the catalytic cracking catalyst, the content of the catalytic cracking aid is 1-20% by weight in terms of weight percentage.
15. A method for catalytic cracking reaction, characterized in that: The method includes: Contacting the crude oil with the catalytic cracking catalyst according to any one of claims 11 to 14 in a catalytic cracking reactor to carry out a catalytic cracking reaction; The temperature of the catalytic cracking reaction is 450-650°C, and the catalyst-oil ratio is 5-20.
16. The method according to claim 15, wherein: The method further comprises: before the feedstock oil contacts the catalytic cracking catalyst, performing reduction pretreatment on the catalytic cracking catalyst or the catalytic cracking aid; The reduction pretreatment comprises: contacting the catalytic cracking catalyst or the catalytic cracking aid with a reducing gas, the time of the reduction pretreatment is 0.5-5 minutes, the temperature of the reduction pretreatment is 650-750° C.; the reducing gas comprises one or more of hydrogen, ethylene and methane.
17. The method according to claim 15, wherein: The method also includes a regeneration process of the catalytic cracking catalyst, wherein the regeneration process includes the following steps: a. Separating the mixed oil obtained from the catalytic cracking reaction to obtain reaction oil gas and spent catalytic material containing spent catalyst and reduced catalytic cracking aid; b. allowing the catalytic material to be regenerated to enter a regenerator for regeneration treatment to obtain a regenerated catalytic material comprising a regenerated catalyst and an oxidized catalytic cracking aid; c. returning the regenerated catalytic material to the catalytic cracking reactor for continued use or returning the regenerated catalytic material to the catalytic cracking reactor for continued use after reduction pretreatment.
18. The method according to claim 17, wherein: Calculated by the weight of copper element, the low-valent copper on the surface of the catalytic cracking aid after the reduction pretreatment accounts for more than 70% of the total weight of the copper element, and the low-valent copper is +1-valent copper.