Aluminum phosphate sol and preparation method thereof, catalytic cracking aid, catalytic cracking catalyst and application thereof, and method for catalytic conversion of hydrocarbon oil
By using a combination of aluminum phosphate sol and modified ZSM-5 zeolite and clay, an efficient catalytic cracking additive is formed, which solves the problem of poor selectivity of propylene in the prior art, and improves the production of propylene and isobutene The rate and concentration improve the overall performance of the catalyst.
Patent Information
- Application Number
- CN202111258118.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-27
AI Technical Summary
The problem of poor selectivity of catalytic cracking additives with existing phosphorus-containing aluminum adhesives in propylene affects the efficiency and yield of the catalytic cracking process.
Aluminum phosphate sol and its preparation method are provided. After hydrolysis of aluminum alkoxide and alcohol solution, polymerization reaction with phosphoric acid is carried out to form an aluminum phosphate sol, and it is used in a catalytic cracking additive, combining modified ZSM-5 zeolite and clay , a catalyst with high purity and uniform particle size is formed.
The yield and concentration of propylene and isobutene in catalytic cracking reaction are improved, and the performance of the catalyst is enhanced, especially in catalytic cracking of heavy oils, which show higher propylene and isobutene yields.
Smart Images

Figure CN116020533B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of aluminum phosphate sol, and in particular to an aluminum phosphate sol and a preparation method thereof, a catalytic cracking aid containing the aluminum phosphate sol, a catalytic cracking catalyst containing the catalytic cracking aid, applications of the catalytic cracking aid and the catalytic cracking catalyst, and a method for catalytic conversion of hydrocarbon oil using the catalytic cracking aid and the catalytic cracking catalyst. Background Art
[0002] Propylene is an important basic chemical raw material. The fluid catalytic cracking process can use heavy oil as raw material and produce more propylene through deep cracking. Therefore, increasing the propylene yield of the catalytic unit is an important way to improve the overall efficiency of the refinery. The addition of catalytic cracking additives to produce more propylene in the catalytic cracking process is widely used due to its advantages of simple operation, flexible reaction and less impact on the entire process. Most propylene additives use ZSM-5 molecular sieves, and in order to further improve the reaction performance of propylene additives, it is usually necessary to modify the ZSM-5 molecular sieve or directly modify the additives, among which phosphorus element modification is the main modification method. The introduction of phosphorus oxides into propylene additives can significantly improve the selectivity for propylene. Therefore, in order to improve the selectivity of propylene, phosphate aluminum gel is currently generally used as a binder.
[0003] CN1796497 discloses a catalytic cracking additive for increasing the production of propylene, characterized in that the additive is composed of 10-65 wt% of modified ZSM-5 molecular sieve, 0-60 wt% of clay, 15-70 wt% of inorganic oxide binder, 0.5-10 wt% of magnesium additive and 0.5-15 wt% of zinc additive on a dry basis, wherein the modified ZSM-5 molecular sieve is modified by phosphorus. The binder, magnesium additive and zinc additive are all calculated as oxides. The additive is applied in the catalytic cracking process, and can significantly increase the propylene concentration in the liquefied gas while increasing the yield of catalytic cracking liquefied gas and improving the octane number of catalytic cracking gasoline.
[0004] CN1872415 discloses a method for preparing a catalytic cracking aid containing ZSM-5 zeolite, characterized in that the ZSM-5 zeolite is crystallized and grown on calcined kaolin, subjected to ion exchange, water washing, drying and / or calcination treatment, and then prepared into a fluidized catalytic cracking aid to improve the performance of the aid, thereby increasing propylene production.
[0005] CN200910237013X discloses a catalytic cracking propylene additive and a preparation method thereof, wherein aluminum phosphate sol is used as both an additive to prepare a binder and a phosphorus modifier. The prepared propylene additive has good wear resistance, higher activity, and lower dry gas and coke yields.
[0006] In order to further improve the propylene yield of the catalytic promoter, the prior art often uses a phosphate aluminum gel binder, but the existing promoter containing the phosphate aluminum gel binder still has the problem of poor propylene selectivity. Summary of the invention
[0007] The purpose of the present invention is to overcome the problem that the existing additives of aluminum phosphate adhesives still have poor propylene selectivity, and to provide an aluminum phosphate sol and a preparation method thereof, a catalytic cracking additive, a catalytic cracking catalyst and its application, and a method for catalytic conversion of hydrocarbon oil.
[0008] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides an aluminum phosphate sol, wherein, on a dry basis, the Al2O3 content of the aluminum phosphate sol is 15-35wt%, and the P2O5 content is 65-85wt%; and the number of colloid particles in the aluminum phosphate sol with a particle size of 30-60nm accounts for more than 90% of the total number of colloid particles in the aluminum phosphate sol.
[0009] A second aspect of the present invention provides a method for preparing aluminum phosphate sol, wherein the method comprises:
[0010] (1) mixing an aluminum alkoxide with an alcohol solution, and subjecting the obtained aluminum alkoxide alcohol solution to a hydrolysis reaction with water to obtain a first slurry;
[0011] (2) stirring the first slurry in an open air to obtain a second slurry;
[0012] (3) subjecting the second slurry to polymerization reaction with phosphoric acid to obtain aluminum phosphate sol.
[0013] The third aspect of the present invention provides an aluminum phosphate sol prepared by the method of the present invention.
[0014] The fourth aspect of the present invention provides a catalytic cracking aid, wherein, based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-55wt% of cracking active components, 5-30wt% of clay and 25-50wt% of a binder; wherein the binder comprises the aluminum phosphate sol provided by the present invention.
[0015] The fifth aspect of the present invention provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, and the auxiliary agent is the catalytic cracking auxiliary agent provided by the present invention.
[0016] A sixth aspect of the present invention provides a use of the catalytic cracking aid or catalytic cracking catalyst provided by the present invention in a catalytic reaction of hydrocarbon oil.
[0017] A seventh aspect of the present invention provides a method for catalytic conversion of hydrocarbon oil, comprising: contacting the hydrocarbon oil with the catalytic cracking aid or catalytic cracking catalyst provided by the present invention for reaction.
[0018] Through the above technical scheme, the present invention provides an aluminum phosphate sol with a specific composition, uniform particle size distribution, high purity, and no other impurities. It can be used as a binder for catalytic cracking catalysts, and the obtained catalyst has good performance.
[0019] The catalytic cracking aid further prepared is used in the hydrocarbon oil catalytic conversion method provided by the present invention, and can be used for hydrocarbon oil catalytic cracking conversion, especially for heavy oil catalytic cracking. While ensuring the strength of the catalyst, it has a higher propylene yield and concentration, and at the same time, the isobutylene yield and concentration are both improved to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is the TEM image of sample PA-4;
[0021] Figure 2 This is the TEM image of sample PA-DB-1. DETAILED DESCRIPTION
[0022] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0023] The first aspect of the present invention provides an aluminum phosphate sol, wherein, on a dry basis, the Al2O3 content of the aluminum phosphate sol is 15-35wt%, and the P2O5 content is 65-85wt%; and the number of particles in the aluminum phosphate sol with a particle size of 30-60nm accounts for more than 90% of the total number of particles in the aluminum phosphate sol.
[0024] In the aluminum phosphate sol provided by the present invention, the particle size of the colloid particles is the size of the projection of the colloid particles, which is equal to the diameter of the largest circumscribed circle of the projection surface and can be measured by TEM.
[0025] In the present invention, the aluminum phosphate sol preferably does not contain chlorine and nitrate. The aluminum phosphate sol also contains water.
[0026] In some embodiments of the present invention, preferably, the aluminum phosphate sol has an Al2O3 content of 19-31wt% and a P2O5 content of 69-81wt% on a dry basis; and the number of particles with a particle size of 30-60nm in the aluminum phosphate sol is 90-100% of the total number of particles in the aluminum phosphate sol. The aluminum phosphate sol with the above particle size can have a relatively uniform mesoporous structure, and can be further used to obtain a catalytic cracking aid that can provide a technical effect of improving propylene selectivity.
[0027] In some embodiments of the present invention, preferably, in the aluminum phosphate sol, the molar ratio of P:Al is 1.6-3:1, preferably 2-3:1. The above elemental composition can be determined by XRF fluorescence analysis method (RIPP 117-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990)).
[0028] In some embodiments of the present invention, preferably, the solid content of the aluminum phosphate sol is 5-35wt%, preferably 10-30wt%. The solid content refers to the total mass content of Al2O3 and P2O5 in the aluminum phosphate sol, which can be determined by the method of calcination at 800°C for 1h.
[0029] In some embodiments of the present invention, preferably, the viscosity of the aluminum phosphate sol is 1500-4000 mPa·s, preferably 2000-3000 mPa·s. Viscosity refers to dynamic viscosity, which can be measured by a Thermo Scientific HAAKE VT550 rotational viscometer, using a 3# rotor, at 20°C and a shear rate of 2900 r / min.
[0030] The aluminum phosphate sol with the above composition and performance parameters provided by the present invention can have high purity, uniform particle size distribution of the colloid particles, the diameter of the colloid particles is mainly concentrated between 30-60nm, high purity, and does not contain other impurities. The prepared catalyst has a large pore volume, which is conducive to being used as a catalytic cracking aid in the catalytic cracking reaction of hydrocarbon oil to obtain products, thereby increasing the concentration of propylene and isobutylene in liquefied petroleum gas.
[0031] A second aspect of the present invention provides a method for preparing aluminum phosphate sol, wherein the method comprises:
[0032] (1) mixing an aluminum alkoxide with an alcohol solution, and subjecting the obtained aluminum alkoxide alcohol solution to a hydrolysis reaction with water to obtain a first slurry;
[0033] (2) stirring the first slurry in an open air to obtain a second slurry;
[0034] (3) subjecting the second slurry to polymerization reaction with phosphoric acid to obtain aluminum phosphate sol.
[0035] In some embodiments of the present invention, step (1) is used to generate a hydrolysis reaction to generate aluminum hydroxyl alcohol, which is subsequently polymerized through the hydroxyl group to provide bonding properties. Preferably, in step (1), the mixing temperature is ≤35°C, preferably 10-35°C; the mixing time is more than 15 minutes, preferably 15-30 minutes.
[0036] The amounts of the raw materials, aluminum alkoxide, alcohol solution and water involved in the hydrolysis reaction are limited to achieve the desired composition of the aluminum phosphate sol. In some embodiments of the present invention, preferably, the mass ratio of the alcohol solution to the aluminum alkoxide is 1-4:1, preferably 1-2:1.
[0037] In some embodiments of the present invention, preferably, the molar ratio of the aluminum alkoxide to water is 1:3-200, preferably 1:60-150.
[0038] In some embodiments of the present invention, preferably, the aluminum alkoxide is selected from aluminum isopropoxide and / or aluminum sec-butoxide, and the alcohol solution is selected from a solution of at least one of methanol, ethanol, ethylene glycol, 1-propanol and glycerol.
[0039] In the present invention, the water may be acidic water, i.e. decationized water, preferably with a pH value of 3-5 and a sodium oxide content of <5 ppm by mass.
[0040] In some embodiments of the present invention, preferably, the temperature of the hydrolysis reaction is 50-100°C, preferably 50-80°C; the time of the hydrolysis reaction is more than 1.5h, preferably 1.5-3h.
[0041] In some embodiments of the present invention, preferably, the hydrolysis reaction process comprises: mixing the aluminum alkoxide alcohol solution with water in batches at least one step, and heating to the temperature of the hydrolysis reaction for reflux stirring. The aluminum alkoxide alcohol solution may be added to water in batches, or water may be added to the aluminum alkoxide alcohol solution in batches.
[0042] In some embodiments of the present invention, preferably, the interval time of the batch mixing is 5-20 minutes, so that the hydrolysis reaction can be carried out more fully, the reaction can be controlled within a reasonable reaction process, and the reaction can generate hydroxyl alcohol aluminum without generating Al(OH)3 precipitation.
[0043] In some embodiments of the present invention, step (2) is used to evaporate the solvent alcohol in the first slurry. Preferably, in step (2), the temperature of the open stirring is not more than 100°C, preferably 60-95°C; the time of the open stirring is not less than 30 minutes, preferably 1-2 hours.
[0044] In some embodiments of the present invention, step (3) is used to generate an aluminum phosphate sol having adhesive properties in the second slurry through the polymerization reaction. Preferably, in step (3), the feeding of the second slurry and the phosphoric acid satisfies that the molar ratio of Al in the second slurry to P in the phosphoric acid satisfies 1.6-3:1, preferably 2-3:1.
[0045] In some embodiments of the present invention, preferably, the phosphoric acid is added to the polymerization reaction in one or two steps; preferably, the phosphoric acid is added in two steps, and more preferably, the phosphorus introduced by the phosphoric acid added in the first step accounts for 3 / 7-3 / 4 of the total weight of the phosphorus introduced by the phosphoric acid, preferably 3 / 5-3 / 4. Adding the phosphoric acid in steps can achieve the effect of reasonably controlling the reaction process.
[0046] In some embodiments of the present invention, preferably, the polymerization reaction temperature is 50-80° C., and the polymerization reaction time is more than 30 min, preferably 30-120 min, and more preferably 60-90 min.
[0047] The third aspect of the present invention provides an aluminum phosphate sol prepared by the method of the present invention.
[0048] In some embodiments of the present invention, preferably, the solid content of the aluminum phosphate sol is 5-35wt%, preferably 10-30wt%.
[0049] Preferably, the viscosity of the aluminum phosphate sol is 1500-4000 mPa·s, preferably 2000-3000 mPa·s.
[0050] In some embodiments of the present invention, preferably, the composition of the prepared aluminum phosphate sol is as described above and will not be repeated herein.
[0051] The fourth aspect of the present invention provides a catalytic cracking aid, wherein, based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-50wt% of cracking active components, 5-30wt% of clay and 25-50wt% of a binder; wherein the binder comprises the aluminum phosphate sol provided by the present invention.
[0052] In some embodiments of the present invention, preferably, the cracking active component is selected from at least one of shape selective zeolite, MCM zeolite and L zeolite, preferably shape selective zeolite.
[0053] Preferably, the framework type of the shape-selective zeolite is an MFI structure, preferably a ZSM-5 zeolite, more preferably a modified ZSM-5 zeolite or a HZSM-5 zeolite.
[0054] Preferably, the modifying element contained in the modified ZSM-5 zeolite is selected from at least one of P, Fe, Co, Mn, Ni, Ga, Zn, Cu, Ti, K, Mg and RE, preferably selected from at least one of P, Fe, Mn, Ga, Cu and RE.
[0055] Preferably, in the modified ZSM-5 zeolite, the content of the modifying element is ≤15wt%.
[0056] Preferably, the molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 20-50, preferably 22-32.
[0057] In the present invention, the above-mentioned modifying elements contained in the modified ZSM-5 zeolite can be added in a step-by-step manner. For example, at least one of ZRP-1, ZRP-5, ZSP-3, ZSP-4 and MPZ molecular sieves is selected, and then other required modifying elements are added. The above-mentioned molecules can be commercially available, such as the ZRP-1 molecular sieve provided by the Qilu Branch of Sinopec Catalyst Co., Ltd., which can contain P modification. Other required modifying elements, such as Fe element, are added to the ZRP-1 molecular sieve as needed.
[0058] In some embodiments of the present invention, preferably, the binder further comprises other binders, and the other binders are selected from at least one of alumina sol, pseudo-boehmite and silica sol;
[0059] In some embodiments of the present invention, preferably, based on the total dry weight of the binder, the content of the other binders in the binder is 0-40 wt %, and the content of the aluminum phosphate sol is 60-100 wt %.
[0060] In some embodiments of the present invention, preferably, based on the total dry weight of the catalytic cracking aid, the content of the aluminum phosphate sol is 24-40wt%, preferably 28-40wt%.
[0061] In some embodiments of the present invention, preferably, the clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay, preferably selected from at least one of kaolin, metakaolin and diatomaceous earth.
[0062] The present invention also provides a method for preparing the above catalytic cracking aid, comprising: mixing cracking active components, a binder, clay and water to form a slurry, drying and roasting, and then washing and drying after washing to obtain the catalytic cracking aid.
[0063] Wherein, the cracking active component can be as described above, preferably a modified ZSM-5 zeolite. It can be modified by multiple steps so that the modified ZSM-5 zeolite contains the modifying elements required by the present invention. Commercially available, such as ZRP-1 molecular sieve, already contains the P element, and then the molecular sieve is contacted with an aqueous solution of a compound containing the modifying element required by the present invention for modification, and the obtained slurry is then mixed with a binder, clay and water. Wherein, in the final modified ZSM-5 zeolite, the content of the modifying element (the total amount of multiple elements) is ≤15wt%, preferably less than or equal to 10wt%.
[0064] In the present invention, the drying temperature is 80-200°C, preferably 80-120°C. The time can be selected according to actual needs, and there is no specific limitation on this. The amount of each component used to form the slurry satisfies the composition of the obtained catalytic cracking aid and meets the requirements of the aforementioned catalytic cracking aid, which will not be repeated here. The roasting conditions can refer to the technical conditions in the art, for example, the roasting temperature can be 500-600°C, and the roasting time can be 4-12h.
[0065] In the present invention, in the preparation method, the washing can be carried out by water washing and / or ammonium washing, and the technical conditions in the art can be referred to, for example, two water washings and one ammonium washing, the water / agent weight ratio (the weight ratio of water to the spherical catalyst particles obtained by roasting) during water washing is (5-10):1, and the temperature is 60-90°C; the ammonium / agent ratio (the weight ratio of ammonium ions in the aqueous solution containing ammonium compounds to the spherical catalyst particles obtained by roasting) during ammonium washing is 1:(50-100). The drying after washing can be, for example, air flow drying or drying, for example, drying at 100-120°C.
[0066] The fifth aspect of the present invention provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, and the auxiliary agent is the catalytic cracking auxiliary agent provided by the present invention.
[0067] It may also be a catalytic cracking aid prepared by the aforementioned preparation method of the catalytic cracking aid.
[0068] The catalytic cracking aid provided by the present invention can be mixed with a catalytic cracking catalyst for use to increase the propylene yield in the catalytic cracking reaction product.
[0069] In some embodiments of the present invention, preferably, based on the total weight of the catalytic cracking catalyst, the content of the main catalyst in the catalytic cracking catalyst is 80-95wt%, preferably 85-92wt%; the content of the auxiliary agent is 5-20wt%, preferably 8-15wt%.
[0070] The main catalyst may be a conventional catalytic cracking catalyst in the art, which can be purchased commercially, such as a catalyst with the brand name HBC produced by Sinopec Catalyst Co., Ltd.
[0071] The sixth aspect of the present invention provides a use of the catalytic cracking aid or catalytic cracking catalyst provided by the present invention in a catalytic reaction of hydrocarbon oil. The hydrocarbon oil can be selected from petroleum and its various fractions.
[0072] The seventh aspect of the present invention provides a method for catalytic conversion of hydrocarbon oil, comprising: contacting hydrocarbon oil with the catalytic cracking aid or catalytic cracking catalyst provided by the present invention for reaction. The reaction may be a catalytic cracking reaction, and the reaction conditions may include: a reaction temperature of 350-800°C, preferably 450-650°C; and a catalyst-oil ratio of 2-25, preferably 2-6.
[0073] In the present invention, when the catalytic cracking adjuvant or catalytic cracking catalyst containing the above-mentioned aluminum phosphate sol is used to carry out catalytic cracking reaction, the distribution of products that can be obtained by treating the above-mentioned hydrocarbon oil can increase the propylene yield and the propylene concentration in the catalytic cracking liquefied gas. At the same time, the butene yield, especially the isobutylene yield, can be increased, and the isobutylene concentration in the catalytic cracking liquefied gas can be increased. In particular, when used for catalytic cracking of heavy oil, the product has a higher propylene yield and concentration, and at the same time, the isobutylene yield and concentration are both improved to a certain extent.
[0074] In the present invention, the room temperature is 10-25°C.
[0075] The present invention will be described in detail below by way of examples. The specifications of the raw materials used in the examples are as follows:
[0076] Pseudo-boehmite: Shanxi Jinlu of China Aluminum Corporation, Al2O3 content 66.36wt%;
[0077] Concentrated phosphoric acid: chemically pure, concentration 85wt%, produced by Beijing Chemical Plant;
[0078] Aluminum isopropoxide: chemically pure, concentration 98wt%, produced by Thermo Fisher Scientific (China) Co., Ltd.;
[0079] Isopropyl alcohol: chemically pure, concentration 99.5wt%, produced by Tianjin Damao Chemical Reagent Factory;
[0080] Acidic water, decationized water, pH 4.5;
[0081] ZRP-1 molecular sieve: produced by Sinopec Catalyst Co., Ltd., Na2O is 0.06wt%, SiO2 / Al2O3 molar ratio is 25, crystallinity is 87%, P modification, content is 2wt%;
[0082] Industrial catalyst: produced by Sinopec Catalyst Co., Ltd., brand name HBC.
[0083] The components of the catalyst obtained in the examples are determined by calculation based on the feed amounts of the various raw materials.
[0084] Analytical methods:
[0085] (1) The composition of each material was analyzed by XRF fluorescence analysis method (RIPP 117-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990)).
[0086] (2) The size of the colloidal particles was measured using a JEM-2000FX-II transmission electron microscope from Japan Electronics Co., Ltd. The sample was prepared by suspension in distilled water and then quickly fixed by alcohol drying. The accelerating voltage was 120 kV. The average particle size of the colloidal particles was obtained by randomly measuring more than 10 colloidal particle projections in the sample TEM image and taking the average value of the maximum circumscribed circle diameter.
[0087] (3) Viscosity is dynamic viscosity, which was measured using a Thermo Scientific HAAKE VT550 rotational viscometer with a 3# rotor at 20°C and a shear rate of 2900 r / min.
[0088] (4) Pore volume: the total pore volume of the cracking catalyst is measured according to the RIPP 151-90 standard method (see "Petrochemical Analysis Methods" (RIPP Test Methods), edited by Yang Cuiding, Science Press, published in 1990).
[0089] (5) Wear index: The wear index of the cracking catalyst is measured according to the RIPP 29-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method), edited by Yang Cuiding, Science Press, published in 1990).
[0090] In the following examples, the room temperature is 10-25°C.
[0091] Examples 1-5 illustrate the preparation of the aluminum phosphate sol provided by the present invention.
[0092] Example 1
[0093] (1) 31 g of aluminum isopropoxide was dissolved in 31 g of isopropanol solution (the mass ratio of the alcohol solution to aluminum alkoxide was 1), mixed and stirred for 15 min, and then mixed and stirred with 165 g of deionized water for 30 min (the molar ratio of aluminum alkoxide to water was 1:60), and then heated to 80° C. and refluxed and stirred for 2 h to obtain an alcohol solution of aluminum isopropoxide;
[0094] (2) heating the alcohol solution of aluminum isopropoxide to 70° C. and stirring for 2 h in an open state to obtain a second slurry;
[0095] (3) 36 g of phosphoric acid (the molar ratio of P:Al is 2.1) was added to the second slurry, and the mixture was refluxed and stirred at 50° C. for 90 min to carry out polymerization reaction to obtain aluminum phosphate sol, which was named PA-1.
[0096] Example 2
[0097] (1) 23.6 g of aluminum isopropoxide was dissolved in 47.3 g of isopropanol solution (the mass ratio of the alcohol solution to aluminum alkoxide was 2), and the mixture was stirred for 30 min. In addition, 208 g of deionized water was heated to 80° C. (the molar ratio of aluminum alkoxide to water was 1:100), and the above solution was added to the deionized water in two batches, and the mixture was stirred for 15 min, and refluxed for 1.5 h to obtain an alcohol solution of aluminum isopropoxide;
[0098] (2) heating the alcohol solution of aluminum isopropoxide to 95° C. and stirring for 1 h in an open state to obtain a second slurry;
[0099] (3) 28.35 g of phosphoric acid was added to the second slurry, and the mixture was refluxed and stirred at 80° C. for 30 min. Then, 11 g of phosphoric acid (the molar ratio of P:Al was 3.0) was added, and the mixture was refluxed and stirred at 80° C. for 60 min to obtain an aluminum phosphate sol, which was named PA-2.
[0100] Example 3
[0101] (1) 27 g of aluminum isopropoxide was dissolved in 27 g of isopropanol solution (the mass ratio of the alcohol solution to aluminum alkoxide was 1), and the mixture was stirred for 15 min. In addition, 354 g of deionized water was heated to 60° C. (the molar ratio of aluminum alkoxide to water was 1:150), and the mixture was stirred with the above solution for 15 min. The mixture was refluxed and stirred for 1 h to obtain an alcohol solution of aluminum isopropoxide.
[0102] (2) heating the alcohol solution of aluminum isopropoxide to 95° C. and stirring for 1 h in an open state to obtain a second slurry;
[0103] (3) 37.8 g of phosphoric acid (the molar ratio of P:Al is 2.5) was added to the second slurry, and the mixture was refluxed and stirred at 60° C. for 90 min to carry out a polymerization reaction to obtain an aluminum phosphate sol, which was named PA-3.
[0104] Example 4
[0105] (1) 27.3 g of aluminum isopropoxide was dissolved in 109 g of isopropanol solution (the mass ratio of the alcohol solution to aluminum alkoxide was 4), mixed and stirred for 30 min, 354 g of deionized water was heated to 80° C. (the molar ratio of aluminum alkoxide to water was 1:150), 118 g of deionized water was added to the above solution in 3 batches every 10 min, mixed and stirred for a total of 30 min, and refluxed and stirred at 80° C. for 2 h to obtain an alcohol solution of aluminum isopropoxide;
[0106] (2) heating the alcohol solution of aluminum isopropoxide to 90° C. and stirring for 1 h in an open state to obtain a second slurry;
[0107] (3) 28.35 g of phosphoric acid was added to the second slurry, and the mixture was refluxed and stirred at 80° C. for 30 min. Then, 9.4 g of phosphoric acid (the molar ratio of P:Al was 2.5) was added, and the mixture was refluxed and stirred at 80° C. for 60 min to obtain an aluminum phosphate sol, which was named PA-4.
[0108] Example 5
[0109] (1) 37.9 g of aluminum isopropoxide was dissolved in 113.8 g of isopropanol solution (the mass ratio of the alcohol solution to aluminum alkoxide was 3), and the mixture was stirred for 30 min. In addition, 669 g of deionized water was heated to 70° C. (the mass ratio of aluminum alkoxide to water was 1:220), and the mixture was mixed with the above solution and stirred for 15 min. The mixture was refluxed and stirred for 5 h to obtain an alcohol solution of aluminum isopropoxide.
[0110] (2) heating the alcohol solution of aluminum isopropoxide to 80° C. and stirring for 1 h in an open state to obtain a second slurry;
[0111] (3) 25.2 g of phosphoric acid was added to the second slurry, and the mixture was refluxed and stirred at 75° C. for 30 min. Then, 8.4 g of phosphoric acid (the molar ratio of P:Al was 1.6) was added, and the mixture was refluxed and stirred at 75° C. for 60 min to obtain an aluminum phosphate sol, which was named PA-5.
[0112] Comparative Example 1
[0113] 21.1 g of pseudo-boehmite (on a dry basis, the same below), 25.8 g of kaolin and 168 g of acidic water were mixed and stirred at 20°C for 30 minutes, 75.6 g of phosphoric acid was added, and then the temperature was raised to 70°C. After the temperature stabilized at 70°C, stirring was continued for 90 minutes to obtain a product recorded as PA-DB-1.
[0114] Comparative Example 2
[0115] 25.5 g of pseudo-boehmite was mixed with 240 g of acidic water at 20°C, stirred and slurried for 30 min, 53 g of phosphoric acid was poured into the pseudo-boehmite slurry and stirred at 60°C for 90 min to obtain a product named PA-DB-2.
[0116] The physicochemical properties of the aluminum phosphate sols obtained in Examples 1-5 and Comparative Examples 1-2 are shown in Table 1, and the TEM image of PA-4 in Example 4 is shown in Figure 1 The TEM image of PA-DB-1 of Comparative Example 1 is shown in Figure 2 .
[0117] Table 1
[0118]
[0119] Note: * The number of particles with a particle size of 30-60 nm in the aluminum phosphate sol is the percentage of the total number of particles in the aluminum phosphate sol.
[0120] From Table 1 and Figure 1 and Figure 2 It can be seen that compared with the comparative example, the aluminum phosphate sol provided by the present invention contains only 15-35wt% Al2O3 and 65-85wt% P2O5 on a dry basis, and the remaining components are water. The comparative example contains impurities such as silicon, gallium, sodium, calcium, and sulfur. The aluminum phosphate sol provided by the present invention has a higher purity. In addition, the diameter of the aluminum phosphate sol particles provided by the present invention is mainly concentrated between 30-60nm, and is composed of Figure 1 and Figure 2 It can be seen that compared with the comparative example, the particle size distribution of the aluminum phosphate sol provided by the present invention is uniform.
[0121] Examples 6-10 illustrate the preparation of the catalytic cracking aid provided by the present invention.
[0122] Example 6
[0123] 156 g of ZRP-1 molecular sieve (on a dry basis, the same below) and 18 g of Fe(NO3)3 were mixed and slurried in 276 g of water for 30 minutes to obtain a molecular sieve slurry; wherein, the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 5.1 wt%, becoming a modified zeolite.
[0124] 21g of kaolin (on a dry basis, the same below), 440g of acidic water, and 9g of pseudo-boehmite (on a dry basis, the same below) were mixed and slurried for 30 minutes, 1.8g of hydrochloric acid was added and stirred for 30 minutes, and then 75g of aluminum phosphate sol PA-4 (on a dry basis, the same below), 33g of aluminum sol (on a dry basis, the same below) and the above molecular sieve slurry were added and stirred for 30 minutes, and spray-dried to prepare a microsphere catalyst.
[0125] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 solution at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, and then washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z1. The proportions are shown in Table 2.
[0126] Example 7
[0127] 126g of ZRP-1 molecular sieve and 18g of Fe(NO3)3 were mixed and slurried in 222g of water for 30 minutes to prepare molecular sieve slurry, wherein the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 6wt%, becoming a modified zeolite.
[0128] 42g kaolin, 484g acidic water and 18g pseudo-boehmite were mixed and slurried for 30min, 3.6g hydrochloric acid was added and stirred for 30min, then 75g aluminum phosphate sol PA-4, 33g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.
[0129] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z2. The proportions are shown in Table 2.
[0130] Example 8
[0131] 96g of shape-selective ZRP-1 molecular sieve and 18g of Fe(NO3)3 were mixed and slurried in 170g of water for 30 minutes to obtain a molecular sieve slurry, wherein the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 7.5wt%, to become a modified zeolite.
[0132] 72g of kaolin, 531g of acidic water and 18g of pseudo-boehmite were mixed and slurried for 30min, 3.6g of hydrochloric acid was added and stirred for 30min, then 75g of aluminum phosphate sol PA-4, 33g of aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to obtain a microsphere catalyst.
[0133] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z3. The proportions are shown in Table 2.
[0134] Example 9
[0135] 126g of ZRP-1 molecular sieve and 18g of Fe(NO3)3 were mixed with 222g of water and beaten for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 6wt%, becoming a modified zeolite.
[0136] 42g kaolin, 484g acidic water and 18g pseudo-boehmite were mixed and slurried for 30min, 3.6g hydrochloric acid was added and stirred for 30min, then 75g aluminum phosphate sol PA-3, 33g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.
[0137] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z4. The proportions are shown in Table 2.
[0138] Example 10
[0139] 135g of ZRP-1 molecular sieve and 12g of Fe(NO3)3 were mixed with 222g of water and slurried for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added made the modifying elements added to the ZRP-1 molecular sieve to be P and Fe, and the content was 4.2wt%, becoming a modified zeolite.
[0140] 40g kaolin, 484g acidic water and 18g pseudo-boehmite were mixed and slurried for 30min, 3.6g hydrochloric acid was added and stirred for 30min, then 72g aluminum phosphate sol PA-5, 30g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.
[0141] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z5. The proportions are shown in Table 2.
[0142] Embodiment 11
[0143] 126g of ZRP-1 molecular sieve and 18g of Fe(NO3)3 were mixed with 222g of water and beaten for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 6wt%, becoming a modified zeolite.
[0144] 36g kaolin, 484g acidic water and 12g pseudo-boehmite were mixed and slurried for 30min, 2.4g hydrochloric acid was added and stirred for 30min, then 96g aluminum phosphate sol PA-4, 24g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.
[0145] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO44 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z6. The proportions are shown in Table 2.
[0146] Comparative Example 3
[0147] 135g of ZRP-1 molecular sieve and 12g of Fe(NO3)3 were mixed with 222g of water and slurried for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added made the modifying elements added to the ZRP-1 molecular sieve to be P and Fe, and the content was 4.2wt%, becoming a modified zeolite.
[0148] 40g kaolin, 484g acidic water and 18g pseudo-boehmite were mixed and slurried for 30min, 3.6g hydrochloric acid was added and stirred for 30min, then 72g aluminum phosphate sol PA-DB-1, 30g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.
[0149] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named DB1. The proportions are shown in Table 2.
[0150] Comparative Example 4
[0151] 135g of ZRP-1 molecular sieve and 12g of Fe(NO3)3 were mixed with 222g of water and slurried for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added made the modifying elements added to the ZRP-1 molecular sieve to be P and Fe, and the content was 4.2wt%, becoming a modified zeolite.
[0152] 40g kaolin, 484g acidic water and 18g pseudo-boehmite were mixed and slurried for 30min, 3.6g hydrochloric acid was added and stirred for 30min, then 72g aluminum phosphate sol PA-DB-2, 30g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.
[0153] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named DB2. The proportions are shown in Table 2.
[0154] Table 2
[0155]
[0156]
[0157] Note: *The modified zeolite is ZRP-1 molecular sieve (already containing P modification, P content is 2wt%) and then modified with Fe.
[0158] ** is the amount of Fe added in the modified zeolite.
[0159] Catalyst reaction evaluation method:
[0160] Z1-Z6, DB1-DB2 and industrial catalyst were mixed in a mass ratio of 1:9 to obtain catalysts C1-C6 and D1-D2. The composition of the industrial catalyst is shown in Table 3.
[0161] Table 3
[0162]
[0163] The composition of the catalytic feedstock oil is shown in Table 4.
[0164] Table 4
[0165]
[0166]
[0167] The catalytic cracking catalysts C1-C6 and D1-D2 prepared above were aged at 800°C and 100% steam for 15 h, respectively, and then filled into a small fixed fluidized bed ACE device (purchased from KTI, USA), with a filling amount of 9 g each. Then, at a reaction temperature of 510°C and a weight hourly space velocity of 12 h -1 The catalyst-oil ratio (weight) was 6, and the catalytic raw oil was injected into the ACE device for catalytic cracking reaction. The reaction results are shown in Table 5.
[0168] The composition of the reaction products is analyzed, including dry gas, liquefied gas, gasoline, diesel, heavy oil and coke, and the catalytic cracking reaction conversion rate of the feedstock oil is calculated according to the following formula:
[0169]
[0170] Liquefied gas contains propylene and C4 olefins. The composition of C4 olefins includes: 1-butene, isobutylene, cis-2-butene and trans-2-butene.
[0171]
[0172]
[0173] Table 5
[0174]
[0175]
[0176] As can be seen from Table 5, the additive prepared by using the aluminum phosphate sol provided by the present invention can have a higher distribution of high value-added products while ensuring the performance and strength of the catalyst (larger pore volume, lower wear index), can increase the propylene yield, and improve the propylene concentration in the catalytic cracking liquefied gas. At the same time, it can increase the 1-butene yield, especially the isobutylene yield, and increase the isobutylene concentration in the catalytic cracking liquefied gas.
[0177] The additive provided by the present invention, compared with the additive prepared by aluminum phosphate sol provided by the prior art (as shown in Comparative Examples 3 and 4), has higher propylene yield, 1-butene and isobutylene yield under the same formula (other components are the same) and has better economic value. When the molecular sieve content is low (such as Example 8 compared with Examples 6 and 7), it can also ensure better propylene yield and 1-butene yield (higher than the comparative example).
[0178] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. An aluminum phosphate sol, characterized in that The aluminum phosphate sol is calculated on a dry basis, and the Al2O3 content of the aluminum phosphate sol is 15-35wt%, the P2O5 content is 65-85wt%, and the total content of Al2O3 and P2O5 is 100wt%; and the number of colloid particles with a particle size of 30-60nm in the aluminum phosphate sol is more than 90% of the total number of colloid particles in the aluminum phosphate sol; in the aluminum phosphate sol, the molar ratio of P:Al is 1.6-3:
1.
2. The aluminum phosphate sol according to claim 1, wherein The aluminum phosphate sol is calculated on a dry basis, and the Al2O3 content of the aluminum phosphate sol is 19-31wt%, and the P2O5 content of the aluminum phosphate sol is 69-81wt%; and the number of particles with a particle size of 30-60nm in the aluminum phosphate sol accounts for 90-100% of the total number of particles in the aluminum phosphate sol.
3. The aluminum phosphate sol according to claim 1 or 2, wherein In the aluminum phosphate sol, the molar ratio of P:Al is 2-3:1; and / or, the solid content of the aluminum phosphate sol is 5-35wt%; And / or, the viscosity of the aluminum phosphate sol is 1500-4000 mPa·s.
4. The aluminum phosphate sol according to claim 3, wherein The solid content of the aluminum phosphate sol is 10-30wt%; And / or, the viscosity of the aluminum phosphate sol is 2000-3000 mPa·s.
5. A method for preparing the aluminum phosphate sol according to any one of claims 1 to 4, characterized in that: The method includes: (1) mixing aluminum alkoxide with an alcohol solution, and subjecting the obtained aluminum alkoxide alcohol solution to a hydrolysis reaction with water to obtain a first slurry; (2) stirring the first slurry in an open air to obtain a second slurry; (3) The second slurry is polymerized with phosphoric acid to obtain aluminum phosphate sol.
6. The method according to claim 5, wherein: In step (1), the mixing temperature is ≤35°C and the mixing time is more than 15 minutes; and / or, the mass ratio of the alcohol solution to the aluminum alkoxide is 1-4:1; and / or, the molar ratio of the aluminum alkoxide to water is 1:3-200; And / or, the temperature of the hydrolysis reaction is 50-100° C.; the time of the hydrolysis reaction is more than 1.5 h; And / or, the hydrolysis reaction process includes: mixing the aluminum alkoxide alcohol solution with water in batches at least in one step, and heating it to the temperature of the hydrolysis reaction and reflux stirring.
7. The method according to claim 6, wherein: In step (1), the mixing temperature is 10-35°C; the mixing time is 15-30 minutes; and / or, the mass ratio of the alcohol solution to the aluminum alkoxide is 1-2:1; and / or, the molar ratio of the aluminum alkoxide to water is 1:60-150; And / or, the temperature of the hydrolysis reaction is 50-80°C; the time of the hydrolysis reaction is 1.5-3h.
8. The method according to claim 6, wherein: The aluminum alkoxide is selected from aluminum isopropoxide and / or aluminum sec-butoxide, and the alcohol solution is selected from at least one of methanol, ethanol, ethylene glycol, 1-propanol and glycerol.
9. The method according to claim 6, wherein: The interval time of the batch mixing is 5-20min.
10. The method according to any one of claims 5 to 9, wherein: In step (2), the temperature of the open stirring is not more than 100°C; the time of the open stirring is not less than 30 minutes; And / or, in step (3), the feeding of the second slurry and the phosphoric acid satisfies that the molar ratio of Al in the second slurry and P in the phosphoric acid satisfies P:Al of 1.6-3:1; And / or, the phosphoric acid is added to the polymerization reaction in one step or two steps; and / or, the polymerization reaction temperature is 50-80° C., and the polymerization reaction time is more than 30 minutes.
11. The method according to claim 10, wherein: In step (2), the temperature of the open stirring is 60-95°C; the time of the open stirring is 1-2h; And / or, in step (3), the feeding of the second slurry and the phosphoric acid satisfies that the molar ratio of Al in the second slurry and P in the phosphoric acid satisfies P:Al of 2-3:1; and / or, the phosphoric acid is added in two steps, the phosphorus introduced in the first step accounting for 3 / 7-3 / 4 of the total weight of the phosphorus introduced by the phosphoric acid; And / or, the polymerization reaction time is 30-120 min.
12. The method according to claim 11, wherein: The phosphorus introduced by adding phosphoric acid in the first step accounts for 3 / 5-3 / 4 of the total weight of phosphorus introduced by the phosphoric acid; And / or, the polymerization reaction time is 60-90 min.
13. A catalytic cracking aid, characterized in that: Based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-55wt% of cracking active components, 5-30wt% of clay and 25-50wt% of a binder; wherein the binder comprises the aluminum phosphate sol according to any one of claims 1-4.
14. The catalytic cracking aid according to claim 13, wherein The cracking active component is at least one selected from the group consisting of shape-selective zeolite, MCM zeolite, and L zeolite; And / or, the binder further comprises other binders, and the other binders are selected from at least one of alumina sol, pseudo-boehmite and silica sol; And / or, the clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay.
15. The catalytic cracking aid according to claim 14, wherein The cracking active component is shape-selective zeolite; and / or, based on the total dry weight of the binder, the content of the other binders in the binder is 0-40wt%, and the content of the aluminum phosphate sol is 60-100wt%; And / or, the clay is selected from at least one of kaolin, metakaolin and diatomaceous earth.
16. The catalytic cracking aid according to claim 14 or 15, wherein: The framework type of the shape-selective zeolite is an MFI structure.
17. The catalytic cracking aid according to claim 16, wherein: The shape selective zeolite is ZSM-5 zeolite.
18. The catalytic cracking aid according to claim 17, wherein The shape selective zeolite is modified ZSM-5 zeolite or HZSM-5 zeolite.
19. The catalytic cracking aid according to claim 18, wherein The modified ZSM-5 zeolite contains at least one modifying element selected from the group consisting of P, Fe, Co, Mn, Ni, Ga, Zn, Cu, Ti, K, Mg and RE.
20. The catalytic cracking aid according to claim 19, wherein The modified ZSM-5 zeolite contains at least one modified element selected from the group consisting of P, Fe, Mn, Ga, Cu and RE.
21. The catalytic cracking aid according to any one of claims 18 to 20, wherein: In the modified ZSM-5 zeolite, the content of the modifying element is ≤15wt%.
22. The catalytic cracking aid according to any one of claims 14-15, 17-20, wherein: The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 20-50.
23. The catalytic cracking aid according to claim 22, wherein: The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 22-32.
24. The catalytic cracking aid according to claim 16, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 20-50.
25. The catalytic cracking aid according to claim 24, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 22-32.
26. The catalytic cracking aid according to claim 21, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 20-50.
27. The catalytic cracking aid according to claim 26, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 22-32.
28. A catalytic cracking catalyst, characterized in that: The catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, wherein the auxiliary agent is the catalytic cracking auxiliary agent described in any one of claims 13-27.
29. The catalytic cracking catalyst according to claim 28, wherein Based on the total weight of the catalytic cracking catalyst, in the catalytic cracking catalyst, the content of the main catalyst is 80-95wt%; and the content of the auxiliary agent is 5-20wt%.
30. The catalytic cracking catalyst according to claim 29, wherein Based on the total weight of the catalytic cracking catalyst, in the catalytic cracking catalyst, the content of the main catalyst is 85-92wt%; and the content of the auxiliary agent is 8-15wt%.
31. Use of the catalytic cracking aid according to any one of claims 13 to 27, or the catalytic cracking catalyst according to any one of claims 28 to 30 in a catalytic reaction of hydrocarbon oil.