Catalytic cracking aid, catalytic cracking catalyst and application thereof, and method for catalytic conversion of hydrocarbon oil

By using a specific composition of aluminum phosphate sol as a binder in the catalytic cracking additive, modifying the Beta zeolite and introducing phosphorus, iron and rare earth metal elements, the poor selectivity of isobutene and high coke yield in the prior art are solved. The problem is to improve the yield and concentration of isobutene in catalytic cracking reaction.

CN116020539BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111258120.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-27
Publication Date
2024-11-12
Estimated Expiration
2041-10-27

AI Technical Summary

Technical Problem

The existing catalytic cracking additives have low concentration of isobutene in liquefied gas, poor selectivity of isobutene and high coke yield.

Method used

A catalytic cracking additive is provided, containing 15-35 wt% of cracking active components, 20-60 wt% of clay and 20-40 wt% of aluminum phosphate sol as binder, and the Al2O3 content of aluminum phosphate sol is 15-35 wt% , the P2O5 content is 65-85 wt%, and the number of rubber particles with a particle size of 30-60 nm is more than 90% of the total number of rubber particles. It is used to introduce phosphorus, iron and rare earth metal elements into the modified Beta zeolite.

Benefits of technology

The yield and concentration of isobutene in the catalytic cracking reaction is improved, the selectivity of carbon tetraolefins is enhanced, the yield of coke is reduced, and the performance of the catalyst is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116020539B_ABST
    Figure CN116020539B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of catalytic cracking aids, and discloses catalytic cracking aids, catalytic cracking catalysts and applications, and a method for catalytic conversion of hydrocarbon oil. Based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 15-35wt% of cracking active components, 20-60wt% of clay, and 20-40wt% of a binder; the binder comprises aluminum phosphate sol; the cracking active components are selected from at least one of aluminum phosphate molecular sieves, silicon aluminum phosphate molecular sieves, hydrogen type and / or modified Beta zeolite; the modified Beta zeolite is introduced with at least one of phosphorus, iron and rare earth metal elements; the aluminum phosphate sol is calculated on a dry basis, and the Al2O3 content in the aluminum phosphate sol is 19-30wt%, and the P2O5 content is 65-85wt%; the number of colloid particles of the aluminum phosphate sol with a particle size of 30-60nm is more than 90% of the total number of colloid particles of the aluminum phosphate sol. The present invention provides a catalytic cracking aid prepared from aluminum phosphate sol, which is used for heavy oil catalytic cracking and has a higher yield and concentration of C4 olefins, especially the yield and concentration of isobutylene are improved to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalytic cracking aids, and in particular to an aluminum phosphate sol and a preparation method thereof, a catalytic cracking aid containing the aluminum phosphate sol, a catalytic cracking catalyst containing the catalytic cracking aid, applications of the catalytic cracking aid and the catalytic cracking catalyst, and a method for catalytic conversion of hydrocarbon oil using the catalytic cracking aid and the catalytic cracking catalyst. Background Art

[0002] With the rapid development of petrochemical industry, the world is demanding C 4 The demand for olefins is increasing year by year. Fluid catalytic cracking is a 4 One of the important processes for olefins, for most catalytic cracking units, adding additives is an effective technical approach to increase the production of light olefins. Changing the performance of catalysts / additives to achieve more light olefins has the technical advantages of flexible operation, economic feasibility, and quick results. However, the existing technology is not effective in increasing the concentration of isobutylene in liquefied gas. From the perspective of isobutylene generation and reaction chemistry in the FCC process, beta molecular sieve is an effective active component, and phosphorus compounds are introduced into the matrix to increase the catalyst's C 4 In this regard, a variety of molecular sieve modification and high-yield propylene catalytic cracking catalyst / auxiliary agent preparation technologies have been developed at home and abroad and have been applied to a certain extent.

[0003] US4837396 discloses a catalyst containing beta zeolite and Y zeolite, and containing a metal ion compound as a stabilizer to improve the hydrothermal stability and mechanical strength of the catalyst. The stabilizer can be [Al 2 (OH) 5 Cl] x , or Al 3 Zr(OH) 9 Cl 4 The stabilizer can directly react with the beta zeolite or can be added during the preparation of the catalyst.

[0004] US6355591 discloses a catalytic cracking aid, which contains 4-20% aluminum phosphate, 1-40% ZSM-5, beta and a mixture thereof, and 40-90% clay, and can increase LPG production. The preparation method of aluminum phosphate is as follows: concentrated phosphoric acid is diluted with deionized water, and aluminum powder is added to dissolve, wherein Al and PO 4 The molar ratio is 1:3, and the pH is less than 2.0. The prepared aluminum phosphate is mixed with kaolin, then mixed into the molecular sieve slurry, and finally sprayed into shape. From the patent claims, the additive does not contain other binders and other inorganic oxides except aluminum phosphate. In addition, the preparation method and performance of the additive containing beta zeolite are not given in the examples of the patent.

[0005] CN1055105C discloses a catalytic cracking catalyst for producing more isobutylene and isopentene. The catalyst is composed of three zeolite components and a carrier: 6-30 wt% of a five-membered ring high-silicon zeolite containing phosphorus and rare earth; 5-20 wt% of USY zeolite; 1-5 wt% of beta zeolite; 30-60 wt% of clay; and 15-30 wt% of an inorganic oxide. The preparation method is: adding a homogenized molecular sieve slurry to a carrier slurry, beating, filtering, drying, and molding to obtain a catalyst product. The catalyst has the characteristics of producing more isobutylene and isopentene under the process conditions of catalytic cracking, and can also co-produce high-octane gasoline.

[0006] CN104946301A discloses a catalytic conversion method for increasing the concentration of light olefins, comprising contacting hydrocarbon oil with a cracking catalyst in a reactor comprising two reaction zones to carry out primary and secondary reactions, wherein the cracking catalyst contains a cracking aid, and the aid includes a beta molecular sieve containing phosphorus and transition metals. The catalytic conversion method for increasing the concentration of light olefins provided by the patent can increase the concentration of ethylene in catalytic cracking dry gas and increase the concentrations of propylene and isobutylene in liquefied gas.

[0007] However, the product distribution obtained when catalytic cracking is carried out using the above-mentioned additives is still not ideal. Summary of the invention

[0008] The purpose of the present invention is to overcome the problems that the existing additives containing phosphorus aluminum gel binder still have low isobutylene concentration in the liquefied gas obtained by catalytic cracking, poor isobutylene selectivity and high coke yield, and to provide a catalytic cracking additive, a catalytic cracking catalyst and its application and a method for catalytic conversion of hydrocarbon oil.

[0009] In order to achieve the above object, the first aspect of the present invention provides a catalytic cracking aid, wherein, based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 15-35wt% of a cracking active component, 20-60wt% of clay and 20-40wt% of a binder; wherein the binder comprises aluminum phosphate sol;

[0010] Wherein, the cracking active component is selected from at least one of aluminum phosphate molecular sieve, silicon aluminum phosphate molecular sieve, hydrogen type and / or modified Beta zeolite; the modification is the introduction of at least one of phosphorus, iron and rare earth metal elements into Beta zeolite;

[0011] The aluminum phosphate sol is calculated on a dry basis. In the aluminum phosphate sol, Al 2 O 3 The content is 15-35wt%, P 2 O 5The content is 65-85wt%; and the number of particles with a particle size of 30-60nm in the aluminum phosphate sol is more than 90% of the total number of particles in the aluminum phosphate sol.

[0012] The second aspect of the present invention provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, and the auxiliary agent is the catalytic cracking auxiliary agent provided by the present invention.

[0013] The third aspect of the present invention provides a use of the catalytic cracking aid or catalytic cracking catalyst provided by the present invention in a catalytic reaction of hydrocarbon oil.

[0014] A fourth aspect of the present invention provides a method for catalytic conversion of hydrocarbon oil, comprising: contacting the hydrocarbon oil with the catalytic cracking aid or catalytic cracking catalyst provided by the present invention for reaction.

[0015] Through the above technical scheme, the present invention provides an aluminum phosphate sol with a specific composition, uniform particle size distribution, high purity, and no other impurities. It can be used as a binder for catalytic cracking catalysts, and the obtained catalyst has good performance.

[0016] The catalytic cracking aid further prepared is used in the hydrocarbon oil catalytic conversion method provided by the present invention, and can be used for the catalytic cracking conversion of hydrocarbon oil, especially for the catalytic cracking of heavy oil. While ensuring the strength of the catalyst, it has a higher yield and concentration of C4 olefins, especially the yield and concentration of isobutylene are improved to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is the TEM image of sample PA-4;

[0018] Figure 2 This is the TEM image of sample PA-DB-1. DETAILED DESCRIPTION

[0019] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0020] The first aspect of the present invention provides a catalytic cracking aid, wherein, based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 15-35wt% of a cracking active component, 20-60wt% of clay and 20-40wt% of a binder; wherein the binder comprises aluminum phosphate sol;

[0021] Wherein, the cracking active component is selected from at least one of aluminum phosphate molecular sieve, silicon aluminum phosphate molecular sieve, hydrogen type and / or modified Beta zeolite; the modification is the introduction of at least one of phosphorus, iron and rare earth metal elements into Beta zeolite;

[0022] The aluminum phosphate sol is calculated on a dry basis. In the aluminum phosphate sol, Al 2 O 3 The content is 15-35wt%, P 2 O 5 The content is 65-85wt%; and the number of particles with a particle size of 30-60nm in the aluminum phosphate sol is more than 90% of the total number of particles in the aluminum phosphate sol.

[0023] In the aluminum phosphate sol provided by the present invention, the particle size of the colloid particles is the size of the projection of the colloid particles, which is equal to the diameter of the largest circumscribed circle of the projection surface and can be measured by TEM.

[0024] In the present invention, the aluminum phosphate sol preferably does not contain chlorine and nitrate. The aluminum phosphate sol also contains water.

[0025] In some embodiments of the present invention, preferably, the aluminum phosphate sol is calculated on a dry basis, and in the aluminum phosphate sol, Al 2 O 3 The content is 19-31wt%, P 2 O 5 The content is 69-81wt%; and the number of the colloid particles of the aluminum phosphate sol with a particle size of 30-60nm is 90-100% of the total number of the colloid particles of the aluminum phosphate sol. The aluminum phosphate sol with the above-mentioned particle size can have a relatively uniform mesoporous structure, and can be further used to obtain a catalytic cracking aid that can provide a technical effect of improving the selectivity of carbon four olefins.

[0026] In some embodiments of the present invention, preferably, in the aluminum phosphate sol, the molar ratio of P:Al is 1.6-3:1, preferably 2-3:1. The above elemental composition can be determined by XRF fluorescence analysis method (RIPP 117-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990)).

[0027] In some embodiments of the present invention, preferably, the solid content of the aluminum phosphate sol is 5-35wt%, preferably 10-30wt%. Solid content refers to the amount of Al in the aluminum phosphate sol. 2 O 3 and P 2 O 5 The total mass content can be determined by the ignition reduction method using calcination at 800°C for 1h.

[0028] In some embodiments of the present invention, preferably, the viscosity of the aluminum phosphate sol is 1500-4000 mPa·s, preferably 2000-3000 mPa·s. Viscosity refers to dynamic viscosity, which can be measured by a Thermo Scientific HAAKE VT550 rotational viscometer, using a 3# rotor, at 20°C and a shear rate of 2900 r / min.

[0029] The catalytic cracking aid provided by the present invention contains aluminum phosphate sol having the above physical and chemical properties, which can help improve C 4 The selectivity of olefins is high, and the yield of isobutylene in the obtained liquefied gas product is high.

[0030] In some embodiments of the present invention, preferably, the method for preparing the aluminum phosphate sol comprises:

[0031] (1) mixing an aluminum alkoxide with an alcohol solution, and subjecting the obtained aluminum alkoxide alcohol solution to a hydrolysis reaction with water to obtain a first slurry;

[0032] (2) stirring the first slurry in an open air to obtain a second slurry;

[0033] (3) subjecting the second slurry to a polymerization reaction with phosphoric acid to obtain aluminum phosphate sol.

[0034] In some embodiments of the present invention, step (1) is used to generate a hydrolysis reaction to generate aluminum hydroxyl alcohol, which is subsequently polymerized through the hydroxyl group to provide bonding properties. Preferably, in step (1), the mixing temperature is ≤35°C, preferably 10-35°C; the mixing time is more than 15 minutes, preferably 15-30 minutes.

[0035] The amounts of the raw materials, aluminum alkoxide, alcohol solution and water involved in the hydrolysis reaction are limited to achieve the desired composition of the aluminum phosphate sol. In some embodiments of the present invention, preferably, the mass ratio of the alcohol solution to the aluminum alkoxide is 1-4:1, preferably 1-2:1.

[0036] In some embodiments of the present invention, preferably, the molar ratio of the aluminum alkoxide to water is 1:3-200, preferably 1:60-150.

[0037] In some embodiments of the present invention, preferably, the aluminum alkoxide is selected from aluminum isopropoxide and / or aluminum sec-butoxide, and the alcohol solution is selected from a solution of at least one of methanol, ethanol, ethylene glycol, 1-propanol and glycerol.

[0038] In the present invention, the water may be acidic water, i.e. decationized water, preferably with a pH value of 3-5 and a sodium oxide content of <5 ppm by mass.

[0039] In some embodiments of the present invention, preferably, the temperature of the hydrolysis reaction is 50-100°C, preferably 50-80°C; the time of the hydrolysis reaction is more than 1.5h, preferably 1.5-3h.

[0040] In some embodiments of the present invention, preferably, the hydrolysis reaction process comprises: mixing the aluminum alkoxide alcohol solution with water in batches at least one step, and heating to the temperature of the hydrolysis reaction for reflux stirring. The aluminum alkoxide alcohol solution may be added to water in batches, or water may be added to the aluminum alkoxide alcohol solution in batches.

[0041] In some embodiments of the present invention, preferably, the interval time of the batch mixing is 5-20 minutes. This allows the hydrolysis reaction to proceed more fully and be controlled within a reasonable reaction process so that aluminum hydroxyl alcohol is generated without generating Al(OH) 3 precipitation.

[0042] In some embodiments of the present invention, step (2) is used to evaporate the solvent alcohol in the first slurry. Preferably, in step (2), the temperature of the open stirring is not more than 100°C, preferably 60-95°C; the time of the open stirring is not less than 30 minutes, preferably 1-2 hours.

[0043] In some embodiments of the present invention, step (3) is used to generate an aluminum phosphate sol having adhesive properties in the second slurry through the polymerization reaction. Preferably, in step (3), the feeding of the second slurry and the phosphoric acid satisfies that the molar ratio of Al in the second slurry to P in the phosphoric acid satisfies 1.6-3:1, preferably 2-3:1.

[0044] In some embodiments of the present invention, preferably, the phosphoric acid is added to the polymerization reaction in one or two steps; preferably, the phosphoric acid is added in two steps, and more preferably, the phosphorus introduced by the phosphoric acid added in the first step accounts for 3 / 7-3 / 4 of the total weight of the phosphorus introduced by the phosphoric acid, preferably 3 / 5-3 / 4. Adding the phosphoric acid in steps can achieve the effect of reasonably controlling the reaction process.

[0045] In some embodiments of the present invention, preferably, the polymerization reaction temperature is 50-80° C., and the polymerization reaction time is more than 30 min, preferably 30-120 min, and more preferably 60-90 min.

[0046] In some embodiments of the present invention, preferably, the cracking active component is hydrogen-type and / or modified Beta zeolite, more preferably modified Beta zeolite, which can be commercially obtained, for example, provided by Qilu Branch of Sinopec Catalyst Co., Ltd. The modified Beta zeolite contains at least one of phosphorus, iron and rare earth elements. The content of the modified element in the modified Beta zeolite is 1-5wt%, preferably 1.1-2wt%. Among them, the SiO of Beta zeolite 2 / Al 2 O 3 The molar ratio is 10-50, preferably 15-30.

[0047] In some embodiments of the present invention, preferably, based on the total dry weight of the catalytic cracking aid, the content of the aluminum phosphate sol is 20-40 wt%.

[0048] In some embodiments of the present invention, preferably, the clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay, preferably selected from at least one of kaolin, metakaolin and diatomaceous earth.

[0049] The present invention also provides a method for preparing the catalytic cracking aid, comprising: forming a slurry from cracking active components, a binder, clay and water, and drying and calcining to obtain the catalytic cracking aid.

[0050] In the present invention, the drying temperature is 80-200°C, preferably 80-120°C. The time can be selected according to actual needs, and there is no specific limitation on this. The amount of each component used to form the slurry satisfies the composition of the obtained catalytic cracking aid and meets the requirements of the aforementioned catalytic cracking aid, which will not be repeated here. The roasting conditions can refer to the technical conditions in the art, for example, the roasting temperature can be 500-600°C, and the roasting time can be 4-12h.

[0051] The second aspect of the present invention provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, and the auxiliary agent is the catalytic cracking auxiliary agent provided by the present invention.

[0052] It may also be a catalytic cracking aid prepared by the aforementioned preparation method of the catalytic cracking aid.

[0053] The catalytic cracking aid provided by the present invention can be mixed with a catalytic cracking catalyst for use to increase the propylene yield of catalytic cracking.

[0054] In some embodiments of the present invention, preferably, based on the total weight of the catalytic cracking catalyst, the content of the main catalyst in the catalytic cracking catalyst is 80-95wt%, preferably 85-92wt%; the content of the auxiliary agent is 5-20wt%, preferably 8-15wt%.

[0055] The main catalyst may be a conventional catalytic cracking catalyst in the art, which can be purchased commercially, such as a catalyst with the brand name HBC produced by Sinopec Catalyst Co., Ltd.

[0056] The third aspect of the present invention provides a use of the catalytic cracking aid or catalytic cracking catalyst provided by the present invention in a catalytic reaction of hydrocarbon oil. The hydrocarbon oil can be selected from petroleum and its various fractions.

[0057] The fourth aspect of the present invention provides a method for catalytic conversion of hydrocarbon oil, comprising: contacting hydrocarbon oil with the catalytic cracking aid or catalytic cracking catalyst provided by the present invention for reaction. The reaction may be a catalytic cracking reaction, and the reaction conditions may include: a reaction temperature of 350-800°C, preferably 450-650°C; an agent-oil ratio of 2-25, preferably 2-6.

[0058] In the present invention, when the catalytic cracking adjuvant or catalytic cracking catalyst containing the above-mentioned aluminum phosphate sol is used to carry out catalytic cracking reaction, the distribution of products that can be obtained by treating the above-mentioned hydrocarbon oil can increase the propylene yield and the propylene concentration in the catalytic cracking liquefied gas. At the same time, the butene yield, especially the isobutylene yield, can be increased, and the isobutylene concentration in the catalytic cracking liquefied gas can be increased. In particular, when used for catalytic cracking of heavy oil, the product has a higher propylene yield and concentration, and at the same time, the isobutylene yield and concentration are both improved to a certain extent.

[0059] In the present invention, the room temperature is 10-25°C.

[0060] The present invention will be described in detail below by way of examples. The specifications of the raw materials used in the examples are as follows:

[0061] Pseudo-boehmite: China Aluminum Group Shanxi Powerhouse, Al 2 O 3 Content 66.36wt%;

[0062] Concentrated phosphoric acid: chemically pure, concentration 85wt%, produced by Beijing Chemical Plant;

[0063] Modified Beta Zeolite: Na 2 O is 0.06%, SiO 2 / Al 2 O 3 21.8, crystallinity 80%, P content 2wt%, Sinopec Catalyst Co., Ltd. Qilu Branch;

[0064] Aluminum isopropoxide: chemically pure, concentration 98wt%, produced by Thermo Fisher Scientific (China) Co., Ltd.;

[0065] Isopropyl alcohol: chemically pure, concentration 99.5wt%, produced by Tianjin Damao Chemical Reagent Factory;

[0066] Acidic water, decationized water, pH 4.5;

[0067] Industrial catalyst: produced by Sinopec Catalyst Co., Ltd., brand name HBC.

[0068] The components of the catalyst obtained in the examples are determined by calculation based on the feed amounts of the various raw materials.

[0069] Analytical methods:

[0070] (1) The composition of each material was analyzed by XRF fluorescence analysis method (RIPP 117-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990)).

[0071] (2) The size of the colloidal particles was measured using a JEM-2000FX-II transmission electron microscope from Japan Electronics Co., Ltd. The sample was prepared by suspension in distilled water and then quickly fixed by alcohol drying. The accelerating voltage was 120 kV. The average particle size of the colloidal particles was obtained by randomly measuring more than 10 colloidal particle projections in the sample TEM image and taking the average value of the maximum circumscribed circle diameter.

[0072] (3) Viscosity is dynamic viscosity, which was measured using a Thermo Scientific HAAKE VT550 rotational viscometer with a 3# rotor at 20°C and a shear rate of 2900 r / min.

[0073] In the following examples, the room temperature is 10-25°C.

[0074] Examples 1-5 illustrate the preparation of the aluminum phosphate sol provided by the present invention.

[0075] Example 1

[0076] (1) dissolving 31 g of aluminum isopropoxide in 31 g of isopropanol solution (the mass ratio of the alcohol solution to the aluminum alkoxide is 1), mixing and stirring for 15 min to obtain an alcohol solution of aluminum isopropoxide, and then mixing and stirring with 165 g of deionized water for 30 min (the molar ratio of the aluminum alkoxide to water is 1:60), heating the solution to 80° C. and refluxing and stirring for 2 h for hydrolysis reaction to obtain a first slurry;

[0077] (2) heating the first slurry to 70° C. and stirring for 2 h in an open state to obtain a second slurry;

[0078] (3) 36 g of phosphoric acid (the molar ratio of P:Al is 2.1) was added to the second slurry, and the mixture was refluxed and stirred at 50° C. for 90 min to carry out a polymerization reaction to obtain an aluminum phosphate sol, which was named PA-1.

[0079] Example 2

[0080] (1) 23.6 g of aluminum isopropoxide was dissolved in 47.3 g of isopropanol solution (the mass ratio of the alcohol solution to the aluminum alkoxide was 2), mixed and stirred for 30 min to obtain an alcohol solution of aluminum isopropoxide, and 208 g of deionized water was heated to 80° C. (the molar ratio of the aluminum alkoxide to water was 1:100), and the above solution was added to the deionized water in two batches at an interval of 5 min, mixed and stirred for 15 min, and refluxed and stirred for 1.5 h for hydrolysis reaction to obtain a first slurry;

[0081] (2) heating the first slurry to 95° C. and stirring for 1 h in an open state to obtain a second slurry;

[0082] (3) 28.35 g of phosphoric acid was added to the second slurry, and the mixture was refluxed and stirred at 80° C. for 30 min. Then, 11 g of phosphoric acid (the molar ratio of P:Al was 3.0) was added, and the mixture was refluxed and stirred at 80° C. for 60 min to carry out polymerization reaction, thereby obtaining aluminum phosphate sol, which was named PA-2.

[0083] Example 3

[0084] (1) 27 g of aluminum isopropoxide was dissolved in 27 g of isopropanol solution (the mass ratio of the alcohol solution to the aluminum alkoxide was 1), and the mixture was stirred for 15 min to obtain an alcohol solution of aluminum isopropoxide. In addition, 354 g of deionized water was heated to 60° C. (the molar ratio of the aluminum alkoxide to water was 1:150), and the mixture was stirred with the above solution for 15 min, and the mixture was refluxed and stirred for 1 h for hydrolysis reaction to obtain a first slurry;

[0085] (2) heating the first slurry to 95° C. and stirring for 1 h in an open state to obtain a second slurry;

[0086] (3) 37.8 g of phosphoric acid (the molar ratio of P:Al is 2.5) was added to the second slurry, and the mixture was refluxed and stirred at 60° C. for 90 min to carry out a polymerization reaction to obtain an aluminum phosphate sol, which was named PA-3.

[0087] Example 4

[0088] (1) 27.3 g of aluminum isopropoxide was dissolved in 109 g of isopropanol solution (the mass ratio of the alcohol solution to aluminum alkoxide was 4), mixed and stirred for 30 min to obtain an alcohol solution of aluminum isopropoxide, 354 g of deionized water was heated to 80° C. (the molar ratio of aluminum alkoxide to water was 1:150), 118 g of deionized water was added to the above solution in three batches every 10 min, mixed and stirred for a total of 30 min, and refluxed and stirred at 80° C. for 2 h to perform a hydrolysis reaction to obtain a first slurry;

[0089] (2) heating the first slurry to 90° C. and stirring for 1 h in an open state to obtain a second slurry;

[0090] (3) 28.35 g of phosphoric acid was added to the second slurry, and the mixture was refluxed and stirred at 80° C. for 30 min. Then, 9.4 g of phosphoric acid (the molar ratio of P:Al was 2.5) was added, and the mixture was refluxed and stirred at 80° C. for 60 min to carry out polymerization reaction, thereby obtaining aluminum phosphate sol, which was named PA-4.

[0091] Example 5

[0092] (1) 37.9 g of aluminum isopropoxide was dissolved in 113.8 g of isopropanol solution (the mass ratio of the alcohol solution to the aluminum alkoxide was 3), and the mixture was stirred for 30 min to obtain an alcohol solution of aluminum isopropoxide. In addition, 669 g of deionized water was heated to 70° C. (the mass ratio of the aluminum alkoxide to water was 1:220), and the mixture was stirred with the above solution for 15 min, and the mixture was refluxed and stirred for 5 h for hydrolysis reaction to obtain a first slurry;

[0093] (2) heating the first slurry to 80° C. and stirring for 1 h in an open state to obtain a second slurry;

[0094] (3) 25.2 g of phosphoric acid was added to the second slurry, and the mixture was refluxed and stirred at 75° C. for 30 min. Then, 8.4 g of phosphoric acid (the molar ratio of P:Al was 1.6) was added, and the mixture was refluxed and stirred at 75° C. for 60 min to carry out polymerization reaction, thereby obtaining aluminum phosphate sol, which was named PA-5.

[0095] Comparative Example 1

[0096] 21.1 g of pseudo-boehmite (on a dry basis, the same below), 25.8 g of kaolin and 168 g of acidic water were mixed and stirred at 20°C for 30 minutes, 75.6 g of phosphoric acid was added, and then the temperature was raised to 70°C. After the temperature stabilized at 70°C, stirring was continued for 90 minutes to obtain a product recorded as PA-DB-1.

[0097] Comparative Example 2

[0098] 25.5 g of pseudo-boehmite was mixed with 240 g of acidic water at 20°C, stirred and slurried for 30 min, 53 g of phosphoric acid was poured into the pseudo-boehmite slurry and stirred at 60°C for 90 min to obtain a product named PA-DB-2.

[0099] The physicochemical properties of the aluminum phosphate sols obtained in Examples 1-5 and Comparative Examples 1-2 are shown in Table 1, and the TEM image of PA-4 in Example 4 is shown in Figure 1 The TEM image of PA-DB-1 of Comparative Example 1 is shown in Figure 2 .

[0100] Table 1

[0101]

[0102]

[0103] Note: * The number of particles with a particle size of 30-60 nm in the aluminum phosphate sol is the percentage of the total number of particles in the aluminum phosphate sol.

[0104] From Table 1 and Figure 1 and Figure 2 It can be seen that compared with the comparative example, the aluminum phosphate sol provided by the present invention contains only 15-35wt% Al 2 O 3 and 65-85wt% P 2 O 5 The remaining components are water. The comparative example contains impurities such as silicon, gallium, sodium, calcium, and sulfur. The aluminum phosphate sol provided by the present invention has a higher purity. In addition, the diameter of the aluminum phosphate sol particles provided by the present invention is mainly concentrated between 30-60nm, and is composed of Figure 1 and Figure 2 It can be seen that compared with the comparative example, the particle size distribution of the aluminum phosphate sol provided by the present invention is uniform.

[0105] Examples 6-10 illustrate the preparation of the catalytic cracking aid provided by the present invention.

[0106] Example 6

[0107] 40 g of modified Beta zeolite (on a dry basis, the same below) was mixed and slurried in 328 g of water for 20 minutes to prepare a molecular sieve slurry, and then 120 g of kaolin (on a dry basis, the same below) was added and mixed and slurried for 30 minutes, and finally 50 g of aluminum phosphate sol PA-3 (on a dry basis, the same below) was added and mixed and slurried for 30 minutes to prepare a catalyst slurry.

[0108] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named Z1. The proportions are shown in Table 2.

[0109] Example 7

[0110] 50 g of modified Beta zeolite was mixed in 307 g of water, and 22.5 g of diammonium hydrogen phosphate was added and mixed and slurried for 20 min, then 100 g of kaolin was added and mixed and stirred for 30 min, and finally 50 g of aluminum phosphate sol PA-4 was added and mixed and stirred for 30 min to prepare a catalyst slurry.

[0111] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named Z2. The proportions are shown in Table 2.

[0112] Example 8

[0113] 40 g of modified Beta zeolite was mixed and slurried in 286 g of water for 20 minutes to obtain a molecular sieve slurry, and then 100 g of kaolin was added and mixed and stirred for 30 minutes, and finally 60 g of aluminum phosphate sol PA-5 was added and mixed and stirred for 30 minutes to obtain a catalyst slurry.

[0114] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named Z3. The proportions are shown in Table 2.

[0115] Example 9

[0116] 60 g of modified Beta zeolite was mixed and slurried in 244 g of water for 20 min to obtain a molecular sieve slurry, and then 60 g of kaolin was added and mixed and stirred for 30 min. Finally, 80 g of aluminum phosphate sol PA-3 was added and mixed and stirred for 30 min to obtain a catalyst slurry.

[0117] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named Z4. The proportions are shown in Table 2.

[0118] Comparative Example 3

[0119] 50 g of modified Beta zeolite (on a dry basis, the same below) was mixed and slurried in 307 g of water for 20 minutes to obtain a molecular sieve slurry, and then 100 g of kaolin (on a dry basis, the same below) was added and mixed and slurried for 30 minutes. Finally, 50 g of aluminum phosphate sol PA-DB-1 (on a dry basis, the same below) was added and mixed and slurried for 30 minutes to obtain a catalyst slurry.

[0120] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named DB1. The proportions are shown in Table 2.

[0121] Comparative Example 4

[0122] 50 g of modified Beta zeolite was mixed and slurried in 307 g of water for 20 min to prepare a molecular sieve slurry, and then 100 g of kaolin was added and mixed and slurried for 30 min. Finally, 50 g of aluminum phosphate sol PA-DB-2 (on a dry basis) was added and mixed and slurried for 30 min to prepare a catalyst slurry.

[0123] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named DB2. The proportions are shown in Table 2.

[0124] Table 2

[0125] Example 6 Example 7 Example 8 Example 9 Comparative Example 3 Comparative Example 4 Additive No. Z1 Z2 Z3 Z4 DB1 DB2 Beta*, wt% 20 25 20 30 25 25 Kaolin, wt% 60 50 50 30 50 50 Aluminum phosphate sol, wt% PA-3 20 40 PA-4 25 PA-5 30 PA-DB-1 25 PA-DB-2 25

[0126] Note: *Modified Beta zeolite, P modified, P content is 2wt%

[0127] Catalyst reaction evaluation method:

[0128] Z1-Z4, DB1-DB2 and industrial catalyst were mixed in a mass ratio of 1:9 to obtain catalysts C1-C4 and D1-D2. The composition of the industrial catalyst is shown in Table 3.

[0129] Table 3

[0130]

[0131] The composition of the catalytic feedstock oil is shown in Table 4.

[0132] Table 4

[0133]

[0134]

[0135] The catalytic cracking catalysts C1-C4 and D1-D2 prepared above were aged at 800°C and 100% steam for 15 h, respectively, and then filled into a small fixed fluidized bed ACE device (purchased from KTI, USA), with a filling amount of 9 g each. Then, at a reaction temperature of 500°C and a weight hourly space velocity of 12 h -1 The catalyst-oil ratio (weight) was 3, and the catalytic raw oil was injected into the ACE device for catalytic cracking reaction. The reaction results are shown in Table 5.

[0136] The composition of the reaction products is analyzed, including dry gas, liquefied gas, gasoline, diesel, heavy oil and coke, and the catalytic cracking reaction conversion rate of the feedstock oil is calculated according to the following formula:

[0137]

[0138] Liquefied gas contains C 4 Olefins, C 4 The composition of olefins includes: 1-butene, isobutylene, cis-2-butene and trans-2-butene.

[0139]

[0140]

[0141] Table 5

[0142]

[0143] As shown in Table 5, the additive prepared by using the aluminum phosphate sol provided by the present invention can have a higher distribution of high value-added products while ensuring the catalyst strength, and improves the C 4 The yield of olefins and C 4 The concentration of olefins, among which the yield and concentration of isobutylene in the system are also improved to a certain extent.

[0144] Compared with the additives prepared by aluminum phosphate sol provided by the prior art (as shown in Comparative Examples 3 and 4), the additives provided by the present invention (such as Examples 7, 8, and 9) have higher C 4 The yield of olefins and C 4 When the molecular sieve content is low (such as when Examples 6, 7, and 8 are compared with Example 9), a better C 4 The yield of olefins and C 4 The concentration of olefins.

[0145] The additive provided by the present invention, when the aluminum phosphate sol provided by the present patent is used alone as a binder, has a higher propylene yield (Example 9) and a significantly higher C 4 Olefin yields and higher isobutylene concentration and selectivity.

[0146] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A catalytic cracking aid, characterized in that: Based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 15-35wt% of a cracking active component, 20-60wt% of clay and 20-40wt% of a binder; wherein the binder comprises aluminum phosphate sol; Wherein, the cracking active component is selected from at least one of aluminum phosphate molecular sieve, silicon aluminum phosphate molecular sieve, hydrogen type and / or modified Beta zeolite; the modification is the introduction of at least one of phosphorus, iron and rare earth metal elements into Beta zeolite; The aluminum phosphate sol is calculated on a dry basis, and the Al2O3 content of the aluminum phosphate sol is 15-35wt%, the P2O5 content is 65-85wt%, and the total content of Al2O3 and P2O5 is 100wt%; and the number of colloid particles with a particle size of 30-60nm in the aluminum phosphate sol is more than 90% of the total number of colloid particles in the aluminum phosphate sol; in the aluminum phosphate sol, the molar ratio of P:Al is 1.6-3:

1.

2. The catalytic cracking aid according to claim 1, wherein The aluminum phosphate sol is calculated on a dry basis, and the Al2O3 content of the aluminum phosphate sol is 19-31wt%, and the P2O5 content of the aluminum phosphate sol is 69-81wt%; and the number of particles with a particle size of 30-60nm in the aluminum phosphate sol accounts for 90-100% of the total number of particles in the aluminum phosphate sol.

3. The catalytic cracking aid according to claim 2, wherein In the aluminum phosphate sol, the molar ratio of P:Al is 2-3:1; and / or, the solid content of the aluminum phosphate sol is 5-35wt%; And / or, the viscosity of the aluminum phosphate sol is 1500-4000 mPa·s.

4. The catalytic cracking aid according to claim 3, wherein The solid content of the aluminum phosphate sol is 10-30wt%; And / or, the viscosity of the aluminum phosphate sol is 2000-3000 mPa·s.

5. The catalytic cracking aid according to any one of claims 1 to 4, wherein: The method for preparing the aluminum phosphate sol comprises: (1) mixing aluminum alkoxide with an alcohol solution, and subjecting the obtained aluminum alkoxide alcohol solution to a hydrolysis reaction with water to obtain a first slurry; (2) stirring the first slurry in an open air to obtain a second slurry; (3) The second slurry is polymerized with phosphoric acid to obtain aluminum phosphate sol.

6. The catalytic cracking aid according to claim 5, wherein In step (1), the mixing temperature is ≤35°C and the mixing time is more than 15 minutes; and / or, the mass ratio of the alcohol solution to the aluminum alkoxide is 1-4:1; and / or, the molar ratio of the aluminum alkoxide to water is 1:3-200; And / or, the temperature of the hydrolysis reaction is 50-100° C.; the time of the hydrolysis reaction is more than 1.5 h; And / or, the hydrolysis reaction process includes: mixing the aluminum alkoxide alcohol solution with water in batches at least in one step, and heating it to the temperature of the hydrolysis reaction and reflux stirring.

7. The catalytic cracking aid according to claim 6, wherein In step (1), the mixing temperature is 10-35°C; the mixing time is 15-30 minutes; and / or, the mass ratio of the alcohol solution to the aluminum alkoxide is 1-2:1; and / or, the molar ratio of the aluminum alkoxide to water is 1:60-150; And / or, the temperature of the hydrolysis reaction is 50-80°C; the time of the hydrolysis reaction is 1.5-3h.

8. The catalytic cracking aid according to claim 6, wherein The aluminum alkoxide is selected from aluminum isopropoxide and / or aluminum sec-butoxide, and the alcohol solution is selected from at least one of methanol, ethanol, ethylene glycol, 1-propanol and glycerol.

9. The catalytic cracking aid according to claim 6, wherein The interval time of the batch mixing is 5-20min.

10. The catalytic cracking aid according to claim 5, wherein: In step (2), the temperature of the open stirring is not more than 100°C; the time of the open stirring is not less than 30 minutes; And / or, in step (3), the feeding of the second slurry and the phosphoric acid satisfies that the molar ratio of Al in the second slurry and P in the phosphoric acid satisfies P:Al of 1.6-3:1; and / or, the phosphoric acid is added to the polymerization reaction in one or two steps; And / or, the polymerization reaction temperature is 50-80° C., and the polymerization reaction time is more than 30 minutes.

11. The catalytic cracking aid according to claim 10, wherein In step (2), the temperature of the open stirring is 60-95°C; the time of the open stirring is 1-2h; And / or, in step (3), the feeding of the second slurry and the phosphoric acid satisfies that the molar ratio of Al in the second slurry and P in the phosphoric acid satisfies P:Al of 2-3:1; and / or, the phosphoric acid is added in two steps, the phosphorus introduced in the first step accounting for 3 / 7-3 / 4 of the total weight of the phosphorus introduced by the phosphoric acid; And / or, the polymerization reaction time is 30-120 min.

12. The catalytic cracking aid according to claim 11, wherein The phosphorus introduced by adding phosphoric acid in the first step accounts for 3 / 5-3 / 4 of the total weight of phosphorus introduced by the phosphoric acid; And / or, the polymerization reaction time is 60-90 min.

13. The catalytic cracking aid according to any one of claims 1 to 4 and 6 to 12, wherein: The clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay.

14. The catalytic cracking aid according to claim 13, wherein The clay is selected from at least one of kaolin, metakaolin and diatomaceous earth.

15. The catalytic cracking aid according to claim 5, wherein: The clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay.

16. The catalytic cracking aid according to claim 15, wherein The clay is selected from at least one of kaolin, metakaolin and diatomaceous earth.

17. A catalytic cracking catalyst, characterized in that: The catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, wherein the auxiliary agent is the catalytic cracking auxiliary agent according to any one of claims 1-16.

18. The catalytic cracking catalyst according to claim 17, wherein Based on the total weight of the catalytic cracking catalyst, in the catalytic cracking catalyst, the content of the main catalyst is 80-95wt%; and the content of the auxiliary agent is 5-20wt%.

19. The catalytic cracking catalyst according to claim 18, wherein Based on the total weight of the catalytic cracking catalyst, in the catalytic cracking catalyst, the content of the main catalyst is 85-92wt%; and the content of the auxiliary agent is 8-15wt%.

20. Use of the catalytic cracking aid according to any one of claims 1 to 16, or the catalytic cracking catalyst according to any one of claims 17 to 19 in a catalytic reaction of hydrocarbon oil.

21. A method for catalytic conversion of hydrocarbon oil, comprising: The hydrocarbon oil is contacted with the catalytic cracking aid described in any one of claims 1 to 16, or with the catalytic cracking catalyst described in any one of claims 17 to 19 for reaction.