Fluidized solidified soil prepared by using engineering waste slag and method thereof

By adding slag micro powder, fly ash and alkali exciter solutions to the project waste slag, fluid solidified soil with good fluidity and self-solidity is prepared, which solves the problems of waste slag disposal and cement requirements, and realizes the Resource-based utilization and environmental protection are suitable for a variety of engineering applications.

CN116023078BActive Publication Date: 2024-11-08NANJING SUYI IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310048435.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-31
Publication Date
2024-11-08
Estimated Expiration
2043-01-31

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively utilize and treat engineering waste soil, and its dehydration treatment costs are high and poses safety risks. At the same time, the cement demand in the construction industry brings problems of high energy consumption and high carbon displacement.

Method used

Flow-state solidified soil is prepared by engineering waste slag, slag powder, fly ash and alkali exciter solutions. Through specific feed ratios and stirring processes, fluid-state solidified soil with good fluidity and self-solidity is formed, and alkali excitation is used. Agent improves the condensation problem of slag and fly ash.

Benefits of technology

Resource reuse of engineering waste slag, reduce cement usage, reduce energy consumption, protect the environment, provide reliable materials suitable for foundation pits, pipeline trenches, mine pit backfills and building foundation reinforcement, and solve waste Difficulty in disposing of waste and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004056612240000051
    Figure BDA0004056612240000051
Patent Text Reader

Abstract

The present invention discloses a fluidized solidified soil and method prepared by using engineering waste slag, wherein the raw materials of the fluidized solidified soil include slag, slag powder, fly ash, alkaline activator solution and water; the feeding mass ratio of the slag powder to the slag is 1:8.0-10.0, the feeding mass ratio of the fly ash to the slag powder is 1:2.0-5.0, and the alkaline activator solution accounts for 10%-15% of the total mass of the slag powder and the fly ash; the preparation steps are: preparing the alkaline activator solution; mixing the slag powder, fly ash and the sieved slag with dry mixing; mixing the prepared alkaline activator solution with the added water, pouring it into the mixed soil body and continuously stirring it to make the fluidity value reach 180mm-220mm. The fluidized soil product prepared by the present invention has good working performance and is widely used. It can be used for backfilling and pouring of various foundation pits, pipeline trenches, and mine pits, and can also be widely used in reinforcement fields such as roadbeds and building foundations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a resource utilization method of engineering waste slag, and in particular to a fluidized solidified soil prepared by utilizing engineering waste slag and a method thereof. Background Art

[0002] In recent years, with the rapid development of urbanization, a large amount of waste soil has been generated during the construction of underground projects such as power tunnels and integrated pipe corridors. The waste soil needs to be dehydrated for reuse, which is costly and still needs to be transported to the receiving site for stacking after dehydration, which not only occupies land resources but also poses safety hazards. At the same time, the development of the construction industry has also led to an increase in the demand for cement year by year, bringing about problems such as high energy consumption and high carbon emissions.

[0003] To this end, based on the preparation principle of fluidized solidified soil, construction waste and industrial waste can be recycled and utilized to meet the requirements of green, low-carbon and sustainable development of saving costs and protecting the environment. However, how to prepare it specifically and how to introduce construction waste while maintaining the good performance of fluidized solidified soil are issues that need to be resolved. Summary of the invention

[0004] Purpose of the invention: The present invention aims to provide a fluidized solidified soil prepared by using engineering waste slag and having good performance; another purpose of the present invention is to provide a method for preparing fluidized solidified soil by using engineering waste slag.

[0005] Technical solution: The fluidized solidified soil of the present invention comprises raw materials including engineering waste soil, slag powder, fly ash, alkaline activator solution and water;

[0006] The mass ratio of the slag powder to the waste slag is 1:8.0-10.0;

[0007] The feed mass ratio of fly ash to slag powder is 1:2.0-5.0;

[0008] The alkali activator solution accounts for 10%-15% of the total mass of the slag powder and fly ash.

[0009] Furthermore, the amount of water added to the raw material and the total amount of water contained in the air-dried slag account for 55%-70% of the total solid mass.

[0010] Furthermore, the organic matter content in the waste soil does not exceed 5wt%. It should be noted that the organic matter in the waste soil will dissolve to form holes, resulting in loose soil, poor soil bearing capacity and stability, and different effects on the incorporation of different engineering materials.

[0011] Furthermore, the slag powder adopts S95 grade granulated blast furnace slag powder. It should be noted that blast furnace slag belongs to a high calcium system with a high calcium oxide content, and alkali-slag cement has problems such as too fast coagulation, difficult to control molding, large shrinkage and easy cracking.

[0012] Furthermore, the fly ash adopts Class F secondary fly ash. It should be noted that currently a large amount of fly ash is produced every year, which not only occupies a large amount of land resources, but also pollutes the surrounding environment. The present invention uses waste slag as the main material, mixes alkali-activated slag and fly ash to prepare fluidized solidified soil, which saves resources and protects the environment.

[0013] Furthermore, Class F low-calcium fly ash belongs to a low-calcium system, and alkali-activated fly ash cement has problems such as low early strength and slow strength development.

[0014] Furthermore, the alkali-activated slag-fly ash simultaneously exerts the potential hydraulicity of slag and the pozzolanic activity of fly ash, can effectively improve the problems existing in alkali-slag cement and alkali-activated fly ash cement, and has a promoting effect on the disposal of waste slag.

[0015] Furthermore, the alkaline activator solution is a mixed alkaline solution containing solid sodium hydroxide and water glass, wherein the solid sodium hydroxide is used to adjust the water glass modulus, and the water glass modulus M is the ratio of the amount of silicon dioxide to the alkali metal oxide substance, and the value is 0.8-1.2.

[0016] Furthermore, the waste slag can be local excavation residue, waste slag, reduced soil from construction solid waste treatment, etc.

[0017] Furthermore, the selected slag is mainly clay and silty clay. When alkali-activated cementitious materials and water are added and stirred, various components in the cementitious materials react strongly with the water in the slag, and calcium silicate hydrate and other alkaline aluminum silicate hydrates are formed from the solution to cause the mixture to solidify and harden.

[0018] The method for preparing fluidized solidified soil using engineering waste slag has the following specific preparation steps:

[0019] (1) using sodium hydroxide to prepare a sodium silicate solution of corresponding modulus as an alkali activator, and leaving it to stand for use;

[0020] (2) crushing the waste soil and removing foreign matter from the soil, sieving the prepared air-dried soil, measuring its moisture content, and then mixing the air-dried soil with slag powder and fly ash;

[0021] (3) mixing the alkaline activator solution prepared in step (1) with water and stirring, and then pouring it into the mixture of step (2), and then continuing to stir evenly until the flow value reaches 180 mm-220 mm;

[0022] (4) The mixed solution is continuously and evenly stirred to finally obtain a fluidized solidified soil with strong fluidity and good self-compacting property.

[0023] Furthermore, in step (1), the preparation conditions of the sodium silicate solution are: solid sodium hydroxide and the sodium silicate solution are mixed and stirred, the mixed solution is stirred until the solution regains its transparency, and then allowed to stand at 25°C ± 2°C for 24h-48h.

[0024] Furthermore, in step (3), the mass of the added water is specifically: m 添 =xm 总 -m 渣土 w; where m 添 is the mass of water to be added; x = 0.55-0.70; m 总 is the sum of dry mass of slag powder and slag soil; m 渣土 is the dry mass of the slag; w is the moisture content of the air-dried slag.

[0025] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the present invention can recycle a large amount of engineering waste slag as resources, and the prepared fluidized solidified soil has a flow value of 180mm-220mm and a 28d unconfined compressive strength of ≥560kPa, which solves the problem of difficult treatment of engineering waste slag. Alkali-activated slag-fly ash is used as a cementitious material, which reduces the amount of cement used and is green and environmentally friendly. At the same time, the fluidized solidified soil prepared from engineering waste slag has a wide range of applications and can be used for backfilling and pouring of various foundation pits, pipeline trenches, and mine pits. It can also be widely used in reinforcement fields such as road subgrades and building foundations. This solution reduces the safety hazards and environmental damage caused by the disposal of engineering waste slag, and can be used as a resource without dehydration. It is beneficial to save energy, protect the ecology, and is in line with the green, low-carbon and sustainable development strategy. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0027] Example 1

[0028] The raw materials of the fluidized solidified soil include engineering waste slag, slag powder, fly ash, alkali activator solution and water;

[0029] The feed ratio of slag powder to slag soil is 1:8.0;

[0030] The feed ratio of fly ash to slag powder is 1:2.0.

[0031] Furthermore, the mixed alkaline solution containing solid sodium hydroxide and water glass accounts for 10% of the total mass of slag powder and fly ash. The solid sodium hydroxide in the mixed alkaline solution is used to adjust the water glass modulus, wherein the water glass modulus M is the ratio of the amount of silicon dioxide to the amount of alkali metal oxide, and the value is 0.8. It should be noted that sodium hydroxide, commonly known as caustic soda, caustic soda, and caustic soda, is a strong alkali with strong corrosiveness. Sodium hydroxide uses commercially available industrial flake caustic soda with a purity of ≥98%.

[0032] Furthermore, the amount of water added to the raw materials and the total amount of water contained in the air-dried slag account for 55% of the total solid mass; adding water appropriately during the mixing process can obtain a product with better workability.

[0033] The preparation method of the fluidized solidified soil comprises the following steps:

[0034] (1) mixing solid sodium hydroxide and sodium silicate solution, preparing a sodium silicate solution of corresponding modulus as an alkali activator, stirring the mixed solution until the solution regains its transparency, and standing it at 25°C ± 2°C for 24-48 hours for use;

[0035] (2) crushing the waste soil and removing foreign matter from the soil, passing the prepared air-dried soil through a 2 mm sieve, measuring its moisture content, and then mixing the air-dried soil with slag powder and fly ash;

[0036] (3) Mix the prepared alkaline activator solution and water and stir for 5 minutes, then pour it into the mixture of step (2), and continue to stir evenly for 3-5 minutes;

[0037] (4) The mixed solution is continuously and evenly stirred to finally obtain a fluidized solidified soil with strong fluidity and good self-compacting property.

[0038] It can be seen from the above scheme that in Example 1 of the present application, construction waste soil is used as backfill material, and slag, fly ash, alkaline activator solution and water are mixed in appropriate proportions to prepare fluidized backfill material, which can not only protect the environment and realize the effective utilization of construction waste soil and industrial waste residue, but also reduce economic costs and save resources.

[0039] Example 2

[0040] The raw materials of the fluidized solidified soil include engineering waste slag, slag powder, fly ash, alkali activator solution and water;

[0041] The feed ratio of slag powder to slag soil is 1:9.0;

[0042] The feed ratio of fly ash to slag powder is 2.0:7.0.

[0043] Furthermore, the mixed alkaline solution containing solid sodium hydroxide and water glass accounts for 12.5% ​​of the total mass of slag powder and fly ash. The solid sodium hydroxide in the mixed alkaline solution is used to adjust the water glass modulus, wherein the water glass modulus M is the ratio of the amount of silicon dioxide to the amount of alkali metal oxide, and the value is 1.0.

[0044] Furthermore, the amount of water added to the raw materials and the total amount of water contained in the air-dried slag account for 62% of the total solid mass; adding water appropriately during the mixing process can obtain a product with better workability.

[0045] The preparation method of the fluidized solidified soil comprises the following steps:

[0046] (1) mixing solid sodium hydroxide and sodium silicate solution, preparing a sodium silicate solution of corresponding modulus as an alkali activator, stirring the mixed solution until the solution regains its transparency, and standing it at 25°C ± 2°C for 24-48 hours for use;

[0047] (2) crushing the waste soil and removing foreign matter from the soil, passing the prepared air-dried soil through a 2 mm sieve, measuring its moisture content, and then mixing the air-dried soil with slag powder and fly ash;

[0048] (3) Mix the prepared alkaline activator solution and water and stir for 5 minutes, then pour it into the mixture of step (2), and continue to stir evenly for 3-5 minutes;

[0049] (4) The mixed solution is continuously and evenly stirred to finally obtain a fluidized solidified soil with strong fluidity and good self-compacting property.

[0050] Example 3

[0051] The raw materials of the fluidized solidified soil include engineering waste slag, slag powder, fly ash, alkali activator solution and water;

[0052] The feed ratio of slag powder to slag soil is 1:10.0;

[0053] The feed ratio of fly ash to slag powder is 1:5.0.

[0054] Furthermore, the mixed alkaline solution containing solid sodium hydroxide and water glass accounts for 15% of the total mass of slag powder and fly ash. The solid sodium hydroxide in the mixed alkaline solution is used to adjust the water glass modulus, wherein the water glass modulus M is the ratio of the amount of silicon dioxide to the amount of alkali metal oxide, and the value is 1.2.

[0055] Furthermore, the amount of water added to the raw materials and the total amount of water contained in the air-dried slag account for 70% of the total solid mass; adding water appropriately during the mixing process can obtain a product with better workability.

[0056] The preparation method of the fluidized solidified soil comprises the following steps:

[0057] (1) mixing solid sodium hydroxide and sodium silicate solution, preparing a sodium silicate solution of corresponding modulus as an alkali activator, stirring the mixed solution until the solution regains its transparency, and standing it at 25°C ± 2°C for 24-48 hours for use;

[0058] (2) crushing the waste soil and removing foreign matter from the soil, passing the prepared air-dried soil through a 2 mm sieve, measuring its moisture content, and then mixing the air-dried soil with slag powder and fly ash;

[0059] (3) Mix the prepared alkaline activator solution and water and stir for 5 minutes, then pour it into the mixture of step (2), and continue to stir evenly for 3-5 minutes;

[0060] (4) The mixed solution is continuously and evenly stirred to finally obtain a fluidized solidified soil with strong fluidity and good self-compacting property.

[0061] After the preparation is completed according to the above preparation method, the finished products prepared in Examples 1-3 need to be tested for fluidity and unconfined compressive strength, as follows:

[0062] 1) Liquidity test

[0063] The fluidity test device consists of a plexiglass plate and a plexiglass double-opening cylinder with a height of 80mm and an inner diameter of 80mm. During the test, first use a rag to wet the inner wall of the cylinder and the surface of the glass plate, and place the cylinder in the middle of the horizontal glass plate; then load the newly mixed fluid soil sample into the cylinder, and continuously vibrate during the loading process to expel bubbles to ensure that the sample is dense, and use a scraper to flatten the surface after filling; after the loading is completed, gently lift the plexiglass cylinder vertically upwards, and after 30 seconds or when the soil sample no longer spreads, use a steel ruler to measure the maximum and minimum diameters of the mixture after it is spread out, and take the average of the two as the flow value. In order to ensure the reliability of the test, each group of samples needs to be tested 2-3 times in parallel, and the average value is taken as the final flow value;

[0064] 2) Unconfined compressive strength test

[0065] The unconfined compressive strength test is carried out in accordance with the "Standard for Geotechnical Experimental Methods" (GB / T50123-2019). The specimen size is Ф39.1mm×80mm, and the specimen is maintained at (20±2)℃ and above 95% humidity for the specified age. The instrument used in the test is the YYW-2 strain-controlled unconfined pressure instrument produced by Nanjing Soil Instrument Factory, with a compression rate of 1.18mm / min. In order to ensure the reliability of the test, each group of specimens needs to be tested 2-3 times in parallel, and the average value is used as the final unconfined compressive strength.

[0066] In the embodiment of the present application, the test qualification standard is:

[0067] 1) The flow value is 180-220mm, which can be modified according to the requirements of the backfill area if there are special needs;

[0068] 2) The unconfined compressive strength after 3 days is >200kPa, the unconfined compressive strength after 7 days is about 300-400kPa, and the unconfined compressive strength after 28 days is ≤500-900kPa, so as to meet the early strength requirements and later excavation requirements.

[0069] The relevant performance test results of fluidized solidified soil are as follows:

[0070] Specific examples 1-3 are the test results of the performance of fluidized solidified soil prepared by the method for preparing fluidized solidified soil with alkali-activated slag-fly ash provided in this scheme.

[0071]

Claims

1. A fluidized solidified soil prepared from engineering waste soil. Features: Its raw materials include waste slag, slag powder, fly ash, alkali activator solution and water; The mass ratio of the slag powder to the waste slag is 1:8.0-10.0; The feed mass ratio of fly ash to slag powder is 1:2.0-5.0; The alkaline activator solution accounts for 10%-15% of the total mass of slag powder and fly ash; The alkaline activator solution is a mixed alkaline solution containing solid sodium hydroxide and water glass. The water glass modulus M is the ratio of the amount of silicon dioxide to the amount of alkali metal oxide, and the value is 0.8-1.

2.

2. The fluidized solidified soil according to claim 1, Features: The amount of water added to the raw materials and the total amount of water contained in the waste slag account for 55%-70% of the total solid mass.

3. The fluidized solidified soil according to claim 1, Features: The organic matter content in the waste soil does not exceed 5wt%.

4. The fluidized solidified soil according to claim 1, Features: The slag powder is S95 grade granulated blast furnace slag powder.

5. The fluidized solidified soil according to claim 1, Features: The fly ash adopts Class F secondary fly ash.

6. A method for preparing the fluidized solidified soil according to any one of claims 1 to 5, Features: Here are the steps: (1) Use sodium hydroxide to prepare a sodium silicate solution of corresponding modulus as an alkali activator, and let it stand for use; (2) crushing the waste soil and removing foreign matter from the soil, sieving the prepared air-dried soil, measuring its moisture content, and then mixing the air-dried soil with slag powder and fly ash; (3) Mix the prepared alkaline activator solution and water, stir, and pour into the mixture of step (2), and continue to stir evenly until the flow value reaches 180 mm-220 mm; (4) The mixed solution is continuously and evenly stirred to finally obtain a fluidized solidified soil with strong fluidity and good self-compacting properties.

7. The method for preparing the fluidized solidified soil according to claim 6, Features: In step (1), the preparation conditions of the sodium silicate solution are: solid sodium hydroxide and sodium silicate solution are mixed and stirred, the mixed solution is stirred until the solution regains its transparency, and then allowed to stand at 25°C ± 2°C for 24h-48h.

8. The method for preparing the fluidized solidified soil according to claim 6, Features: In step (3), the mass of the added water satisfies: m 添 =xm 总 -m 渣土 w; where m 添 is the mass of water to be added; x=0.55-0.70; m 总 is the sum of dry mass of slag powder, fly ash and slag soil; m 渣土 is the dry mass of the slag; w is the moisture content of the air-dried slag.