A reinforced concrete structure repair material and its preparation and use method

Through the combination of cemented materials and rock wool particles and carbonization maintenance technology, the problems of weather resistance and compressive strength of reinforced concrete structure restoration materials are solved, and efficient and environmentally friendly restoration effects are achieved, and waste rock wool and industrial use are used. The exhaust gas improves the economical and environmentally friendly nature of the repair process.

CN116023106BActive Publication Date: 2024-11-22山东京博环保材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211541552.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-11-22
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

The existing reinforced concrete structure restoration materials have problems such as long repair cycle, poor connection degree, high material cost, and easy corrosion, making it difficult to effectively repair concrete cracks and surface damage.

Method used

Repair materials are prepared using gelled materials, rock wool particles and filamentous rock wool raw materials, and carbonization treatment is carried out through carbonization maintenance technology combined with carbon dioxide waste gas to improve the weather resistance, compressive strength and bonding of the repair materials.

Benefits of technology

The weather resistance, compressive strength and bonding of the repair materials of reinforced concrete structures have been significantly improved, the construction process is simplified, the material cost is reduced, and industrial waste is effectively utilized, which has improved environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003978131980000071
    Figure BDA0003978131980000071
  • Figure BDA0003978131980000081
    Figure BDA0003978131980000081
  • Figure BDA0003978131980000091
    Figure BDA0003978131980000091
Patent Text Reader

Abstract

The present invention provides a repair material for reinforced concrete structure and a preparation and use method thereof, which includes the following raw materials by weight: 90-110 parts of cementitious material, 15-25 parts of rock wool, 0.01-0.1 parts of defoaming agent, and 18-24 parts of water. The cementitious material of the present invention has a dense structure after carbonization, high weathering resistance, corrosion resistance, and high compressive strength; the addition of rock wool particles plays an aggregate support role, accelerates carbonization, and improves the degree of carbonization; under the premise that the filamentous rock wool has hydrophobic properties, according to the characteristics of flexible materials, the toughening effect is exerted to improve the compressive strength, and the rock wool has a heat preservation effect, which better solves the problem of difficult treatment and large-scale accumulation of waste rock wool, so that industrial waste can be reasonably and value-added. Utilization; in addition, the carbonization process uses industrial waste gas for carbonization, and the industrial waste gas is value-added, which effectively improves the environmental pollution caused by industrial waste gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building repair, and in particular to a reinforced concrete structure repair material and a preparation and use method thereof. Background Art

[0002] Reinforced concrete structures are widely used in civil engineering. All kinds of engineering structures can be built with reinforced concrete. This is mainly because reinforced concrete structures have many advantages such as good integrity, good moldability, good durability, and good fire resistance. However, they also have disadvantages such as heavy weight, low tensile strength, easy to cause cracking, labor-intensive and long template cycle, and difficult repair. Therefore, defects will appear in buildings over time. For example, if concrete cracks are not repaired in time or repaired improperly, the protection ability of steel bars will be reduced, resulting in accelerated damage and greatly reducing the service life of the building; there are also natural erosion and weathering effects, resulting in missing corners and surface damage of the building; or indentations, damage, and collapse (small scale) in the concrete pavement; if these defects are well repaired in the later maintenance, the life of the building or concrete pavement will be greatly improved.

[0003] In view of the above problems, concrete including silicate cement, sulfate cement, etc. or other mortar materials are often used for repair, but the repair period is long, the connection between the repair material and reinforced concrete / concrete is poor, the material cost is high, secondary aging, corrosion, etc. are caused, in addition, for example, to repair cracks in concrete pavement, V-shaped grooves, connecting grooves, etc. must be set up before construction, and the construction process is cumbersome.

[0004] Therefore, it is very necessary to provide a repair material with good connection between the repair material and the reinforced concrete / concrete and high strength. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a reinforced concrete structure repair material. The reinforced concrete structure repair material provided by the present invention has high weathering resistance, corrosion resistance, and high compressive strength, and the degree of integration of the repair material with the building is good.

[0006] The invention provides a repairing material for a reinforced concrete structure, which comprises the following raw materials in parts by weight: 90-110 parts of a cementitious material, 15-25 parts of rock wool, 0.01-0.1 parts of a defoaming agent, and 18-24 parts of water.

[0007] Preferably, the rock wool is rock wool particles and filamentous rock wool.

[0008] Preferably, the rock wool particles are obtained by granulating waste rock wool or waste building materials; the particle size of the rock wool particles is 0.5 mm to 80 mm.

[0009] Preferably, the filamentous rock wool is obtained by crushing, loosening and combing waste rock wool;

[0010] The method also includes spraying a water repellent on the filamentous rock wool; the concentration of the water repellent is 35% to 45% of a methyl silicate solution.

[0011] Preferably, the cementitious material comprises calcium silicate or calcium-based or magnesium-based industrial solid waste; the calcium silicate comprises one or more of γ-type dicalcium silicate, β-type dicalcium silicate, monocalcium silicate, dicalcium silicate, tricalcium silicate, calcium oxide or calcium hydroxide; the calcium-based or magnesium-based industrial solid waste comprises one or more of steel slag, magnesium slag, carbide slag, phosphogypsum and waste rock powder;

[0012] The defoamer is selected from any one of a high-carbon alcohol defoamer or a polyether defoamer; the high-carbon alcohol defoamer includes one or more of a silicone defoamer, a polyester defoamer, a n-butanol defoamer or a fatty alcohol defoamer; the polyether defoamer includes one or more of a GP-type glycerol polyether, a GPE-type polyoxyethylene polyoxypropylene glycerol ether or a silicone-polyether composite defoamer.

[0013] Preferably, the repair material also includes 1 to 3 parts by weight of ceramic slag and 1 to 3 parts by weight of shell slag.

[0014] The present invention provides a preparation method for a repair material for a reinforced concrete structure according to any one of the above technical solutions, comprising the following steps:

[0015] A) mixing the cementitious material and the rock wool particles to obtain a mixed dry material;

[0016] B) The filamentous rock wool, water and mixed dry materials are mixed and stirred uniformly, and a defoaming agent is added to obtain the product.

[0017] The present invention provides a method for using a repair material for a reinforced concrete structure, comprising:

[0018] The repair material for reinforced concrete structure described in any one of the above technical solutions is used to pour and fill the cracks or damages of the reinforced concrete structure; and then carbonization curing is performed.

[0019] Preferably, the carbonization curing conditions are: carbonization gas: industrial waste gas with a carbon dioxide content of not less than 1%; carbonization temperature 0-45° C., carbonization pressure 0-1 MPa, and carbonization time 1-72 h.

[0020] The present invention provides a repair material for reinforced concrete structures described in any one of the above technical solutions or a repair material prepared by the preparation method described in the above technical solution for use in cracks in reinforced concrete structures, corner chips in concrete, surface damage in concrete, indentations in concrete, collapse in concrete or cracks in concrete.

[0021] Compared with the prior art, the present invention provides a repair material for reinforced concrete structure, which includes the following raw materials by weight: 90-110 parts of cementitious material, 15-25 parts of rock wool, 0.01-0.1 parts of defoaming agent, and 18-24 parts of water. The cementitious material of the present invention has a dense structure after carbonization, high weathering resistance, corrosion resistance, and high compressive strength; the addition of rock wool particles plays an aggregate support role, accelerates carbonization, and improves the degree of carbonization; under the premise that the filamentous rock wool has hydrophobic properties, according to the characteristics of flexible materials, the toughening effect is exerted to improve the compressive strength, and the rock wool has a heat preservation effect, which better solves the problem of difficult treatment and large-scale accumulation of waste rock wool, so that industrial waste can be reasonably and value-added. Utilization; in addition, the carbonization process uses industrial waste gas for carbonization, and the industrial waste gas is value-added, which effectively improves the environmental pollution caused by industrial waste gas. DETAILED DESCRIPTION

[0022] The present invention provides a reinforced concrete structure repair material and a method for preparing and using the same. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar replacements and modifications are obvious to those skilled in the art, and they all fall within the scope of protection of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0023] The invention provides a repairing material for a reinforced concrete structure. The repairing material comprises the following raw materials in parts by weight: 90 to 110 parts of a cementitious material, 15 to 25 parts of rock wool, 0.01 to 0.1 parts of a defoaming agent, and 18 to 24 parts of water.

[0024] The raw materials of the repair material for reinforced concrete structure provided by the present invention include 90 to 110 parts by weight of cementitious material; preferably include 95 to 105 parts by weight; more preferably, it can be 90 parts by weight, 95 parts by weight, 100 parts by weight or 105 parts by weight or any value in between the above two parts.

[0025] The cementitious material of the present invention includes but is not limited to calcium silicate or calcium-based or magnesium-based industrial solid waste; the calcium silicate includes one or more of γ-type dicalcium silicate, β-type dicalcium silicate, monocalcium silicate, dicalcium silicate, tricalcium silicate, calcium oxide or calcium hydroxide; the calcium-based or magnesium-based industrial solid waste includes one or more of steel slag, magnesium slag, carbide slag, phosphogypsum and waste rock powder;

[0026] The raw materials of the repair material for reinforced concrete structure provided by the present invention include 15 to 25 parts by weight of rock wool, and more preferably include 15 to 23 parts by weight.

[0027] According to the present invention, the rock wool is rock wool particles and filamentous rock wool.

[0028] Specifically, the rock wool particles are obtained by granulating waste rock wool or waste building materials; the present invention does not limit waste rock wool or waste building materials, and those familiar to those skilled in the art are sufficient.

[0029] The rock wool particles can be of multi-graded particle sizes, with a particle size of 0.5 mm to 80 mm.

[0030] The filamentous rock wool of the present invention is obtained by crushing, loosening and combing waste rock wool;

[0031] The present invention further comprises spraying a water repellent on the filamentous rock wool; the water repellent concentration is 35% to 45% of a methyl silicate solution.

[0032] After spraying the water-repellent agent, it is dried (not limited to the drying method) to form a water-repellent protective film; under the premise of having water-repellent properties, the filamentous rock wool exerts its toughening effect according to its flexible material characteristics, improves the toughness of the repair material, and improves the flexural strength.

[0033] The raw materials of the repair material for reinforced concrete structure provided by the present invention include 0.01 to 0.1 parts by weight of defoamer; more preferably, 0.02 to 0.09 parts by weight; the defoamer is made of high-carbon alcohols, polyethers and lipids, and is suitable for alkaline environments.

[0034] Specifically, it can be any one of the high-carbon alcohol defoamers or polyether defoamers; the high-carbon alcohol defoamer includes one or more of silicone defoamers, polyester defoamers, n-butanol defoamers or fatty alcohol defoamers; the polyether defoamer includes one or more of GP-type glycerol polyether, GPE-type polyoxyethylene polyoxypropylene glycerol ether or silicone polyether composite defoamers.

[0035] The raw materials of the repair material for reinforced concrete structure provided by the invention include 18 to 24 parts by weight of water.

[0036] The repair material for reinforced concrete structure provided by the present invention preferably further comprises 1 to 3 parts by weight of ceramic slag and 1 to 3 parts by weight of shell slag. The ceramic slag is obtained by crushing ceramic waste materials and waste products, and the shell slag is obtained by crushing shells.

[0037] The above components of the present invention are technical features that they support each other functionally and have an interactive relationship. The synergistic effect of the above components makes the repair material of the present invention highly resistant to weathering, corrosion, and compressive strength, and the degree of integration of the repair material with the building is good.

[0038] The present invention provides a preparation method for a repair material for a reinforced concrete structure according to any one of the above technical solutions, comprising the following steps:

[0039] A) mixing the cementitious material and the rock wool particles to obtain a mixed dry material;

[0040] B) The filamentous rock wool, water and mixed dry materials are mixed and stirred uniformly, and a defoaming agent is added to obtain the product.

[0041] The present invention has clearly described the above components and proportions, which will not be repeated here.

[0042] The present invention firstly mixes the cementitious material and the rock wool particles respectively according to weight fractions to obtain a mixed dry material.

[0043] The present invention does not limit the mixing method, and any method known to those skilled in the art may be used.

[0044] In the mixed dry material, filamentous rock wool and water are added to the mixed dry material prepared in step 1 respectively, and the mixture is stirred evenly and a defoaming agent is added to prepare a repair material.

[0045] The present invention provides a method for using a repair material for a reinforced concrete structure, comprising:

[0046] The repair material for reinforced concrete structure described in any one of the above technical solutions is used to pour and fill the cracks or damages of the reinforced concrete structure; and then carbonization curing is performed.

[0047] According to the size of the cracks or damages in the reinforced concrete structure, the particle size of the multi-graded rock wool particles is determined, and an appropriate amount of the repair material provided by the present invention is taken for pouring or filling. After the pouring or filling is completed, carbonization curing is performed.

[0048] Furthermore, the carbonization curing conditions are: carbonization gas, industrial waste gas with a carbon dioxide content of not less than 1% (including 1%); carbonization temperature 0-45°C, carbonization pressure 0-1MPa, carbonization time 1-72h; the carbonization time is adjusted according to the size of the cracks or damage in the reinforced concrete structure.

[0049] The present invention provides a repair material for reinforced concrete structures described in any one of the above technical solutions or a repair material prepared by the preparation method described in the above technical solution for use in cracks in reinforced concrete structures, corner chips in concrete, surface damage in concrete, indentations in concrete, collapse in concrete or cracks in concrete.

[0050] Positive effects of the present invention:

[0051] (1) The repair material for reinforced concrete structure provided by the present invention has a dense structure of cementitious materials after carbonization, high weathering resistance, corrosion resistance, and high compressive strength; rock wool particles with multi-graded particle sizes can meet the requirements of aggregate support and carbonized pores of different depths and widths, effectively replace sand and gravel, and are more conducive to constructing effective pores, promoting the entry of carbonized gas containing carbon dioxide, increasing the degree of carbonization, and improving mechanical properties; at the same time, since the rock wool particles are wrapped with waste concrete particles after granulation, the rock wool particles themselves also have a certain compressive strength; the filamentous rock wool is obtained from waste rock wool, and the rock wool has been endowed with a certain The water-repellent effect can be achieved by spraying a water-repellent agent on the filamentary rock wool. Under the premise of having water-repellent properties, according to the characteristics of its flexible material, its toughening effect can be exerted to enhance the toughness of the repair material and improve the compressive strength. The rock wool can also play a certain role in thermal insulation. In addition, the selection of rock wool can also solve the problem of the difficulty in handling waste rock wool and the large-scale accumulation, so that industrial waste can be reasonably and value-added. Utilization; in addition, the carbonization process can use industrial waste gas with a carbon dioxide content of not less than 1% for carbonization, so that the industrial waste gas can be value-added and utilized, effectively improving the environmental pollution caused by industrial waste gas and other problems.

[0052] (2) The repair material provided by the present invention is used to repair reinforced concrete structures or other concretes. The construction is simple and fast. After cleaning the location to be repaired, the construction can be carried out at any time. The operation is simple and the construction period is saved. The repair material is well integrated with the building, reducing secondary repairs. In addition, the anti-aging, anti-freeze and corrosion resistance properties are also significantly improved.

[0053] (3) The repair material for reinforced concrete structure provided by the present invention may also be added with ceramic slag and shell slag, which can effectively improve the waterproof effect and effectively solve the problem of processing ceramic waste materials and waste products.

[0054] In order to further illustrate the present invention, an iron supplement effervescent tablet and a preparation method thereof provided by the present invention are described in detail below in conjunction with examples.

[0055] The raw materials or auxiliary materials used in the present invention can be purchased from the market. The cementitious materials involved in the following embodiments and comparative examples are exemplified by steel slag. Although other cementitious materials involved in this application are not disclosed here in sequence, it does not mean that they do not have the effect of the steel slag example.

[0056] Embodiment 1:

[0057] An embodiment of the present invention provides a repair material for a reinforced concrete structure, which includes the following raw materials in parts by weight: 90 parts of steel slag, 10 parts of rock wool particles, 5 parts of filamentous rock wool, 0.01 parts of defoaming agent, and 18 parts of water.

[0058] Take cementitious materials and rock wool particles respectively by weight and mix them evenly to obtain a mixed dry material; add filamentous rock wool and water into the mixed dry material respectively, stir the defoaming agent evenly to obtain slurry, and prepare the repair material; take an appropriate amount of the repair material provided by the present invention for pouring or filling, and perform carbonization curing after the pouring or filling is completed.

[0059] The carbonization curing conditions are as follows: the carbonization gas has a carbon dioxide content of 5% of industrial waste gas; the carbonization temperature is 25° C., the carbonization pressure is 0.1 MPa, and the carbonization time is 2 hours.

[0060] Embodiment 2:

[0061] An embodiment of the present invention provides a repair material for a reinforced concrete structure, which includes the following raw materials in parts by weight: 100 parts of steel slag, 10 parts of rock wool particles, 10 parts of filamentous rock wool, 0.06 parts of defoaming agent, and 21 parts of water.

[0062] Take cementitious materials and rock wool particles respectively by weight and mix them evenly to obtain a mixed dry material; add filamentous rock wool and water into the mixed dry material respectively, stir the defoaming agent evenly to obtain slurry, and prepare the repair material; take an appropriate amount of the repair material provided by the present invention for pouring or filling, and perform carbonization curing after the pouring or filling is completed.

[0063] The carbonization curing conditions are as follows: the carbonization gas has a carbon dioxide content of 5% of industrial waste gas; the carbonization temperature is 25° C., the carbonization pressure is 0.1 MPa, and the carbonization time is 2 hours.

[0064] Embodiment 3:

[0065] An embodiment of the present invention provides a repair material for a reinforced concrete structure, which includes the following raw materials in parts by weight: 110 parts of steel slag, 15 parts of rock wool particles, 10 parts of filamentous rock wool, 0.1 parts of a defoaming agent, and 24 parts of water.

[0066] Take cementitious materials and rock wool particles respectively by weight and mix them evenly to obtain a mixed dry material; add filamentous rock wool and water into the mixed dry material respectively, stir the defoaming agent evenly to obtain slurry, and prepare the repair material; take an appropriate amount of the repair material provided by the present invention for pouring or filling, and perform carbonization curing after the pouring or filling is completed.

[0067] The carbonization curing conditions are as follows: the carbonization gas has a carbon dioxide content of 5% of industrial waste gas; the carbonization temperature is 25° C., the carbonization pressure is 0.1 MPa, and the carbonization time is 2 hours.

[0068] The carbonization time is adjusted according to the extent of cracking or damage in the reinforced concrete structure.

[0069] In Examples 1 to 3, similar damaged grooves of 100mmX100mmX80mm reinforced concrete blocks were repaired under the same conditions. After the repair, the repaired parts of the reinforced concrete blocks were tested for compressive strength, frost resistance, ultraviolet aging test, bonding degree, and salt spray test. The results are shown in Table 1 below:

[0070] Table 1: Experimental results of Examples 1 to 3

[0071]

[0072] Embodiment 4:

[0073] The difference between Example 4 and Example 3 is that the concentration of carbonized gas in the carbonization curing conditions is different. The embodiment of the present invention provides a repair material for reinforced concrete structure, which includes the following raw materials in parts by weight: 110 parts of steel slag, 15 parts of rock wool particles, 10 parts of filamentary rock wool, 0.1 parts of defoaming agent, and 24 parts of water.

[0074] Take cementitious materials and rock wool particles respectively by weight and mix them evenly to obtain a mixed dry material; add filamentous rock wool and water into the mixed dry material respectively, stir the defoaming agent evenly to obtain slurry, and prepare the repair material; take an appropriate amount of the repair material provided by the present invention for pouring or filling, and perform carbonization curing after the pouring or filling is completed.

[0075] The carbonization curing conditions are as follows: the carbonization gas has a carbon dioxide content of 10% of industrial waste gas; the carbonization temperature is 25° C., the carbonization pressure is 0.1 MPa, and the carbonization time is 2 hours.

[0076] The carbonization time is adjusted according to the extent of cracking or damage in the reinforced concrete structure.

[0077] Embodiment 5:

[0078] The difference between Example 5 and Example 3 is that the concentration of carbonized gas in the carbonization curing conditions is different. The embodiment of the present invention provides a repair material for reinforced concrete structure, which includes the following raw materials in parts by weight: 110 parts of steel slag, 15 parts of rock wool particles, 10 parts of filamentary rock wool, 0.1 parts of defoaming agent, and 24 parts of water.

[0079] Take cementitious materials and rock wool particles respectively by weight and mix them evenly to obtain a mixed dry material; add filamentous rock wool and water into the mixed dry material respectively, stir the defoaming agent evenly to obtain slurry, and prepare the repair material; take an appropriate amount of the repair material provided by the present invention for pouring or filling, and perform carbonization curing after the pouring or filling is completed.

[0080] The carbonization curing conditions are as follows: the carbonization gas has a carbon dioxide content of 15% of industrial waste gas; the carbonization temperature is 25° C., the carbonization pressure is 0.1 MPa, and the carbonization time is 2 hours.

[0081] The carbonization time is adjusted according to the extent of cracking or damage in the reinforced concrete structure.

[0082] The difference between Examples 4 and 5 and Example 3 is that the carbonization gas concentrations in the carbonization curing conditions are different; under the same conditions, similar damaged grooves of 100mmX100mmX80mm reinforced concrete blocks were repaired, and after the repair, the compressive strength, frost resistance, ultraviolet aging test, bonding degree, and salt spray test were performed on the repaired parts of the reinforced concrete blocks. The results are shown in Table 2 below:

[0083] Table 2

[0084]

[0085] From the comparison of Examples 3 to 5, it can be seen that with the increase of the carbon dioxide concentration during carbonation curing, the compressive strength gradually increases, indicating that the carbonization effect of the cementitious material is better in an atmosphere with a higher carbon dioxide concentration, and therefore the compressive strength is greater; indicating that the carbonization effect of the cementitious material is better in an atmosphere with a higher carbon dioxide concentration, and therefore the compressive strength is greater.

[0086] Embodiment 6:

[0087] The difference from Example 3 is that the carbonization time is different, and the carbonization time of Example 6 is 6 hours.

[0088] Embodiment 7:

[0089] The difference from Example 3 is that the carbonization time is different, and the carbonization time of Example 6 is 10 hours.

[0090] In Example 6 and Example 7, similar damaged grooves of 100mmX100mmX80mm reinforced concrete blocks were repaired under the same conditions as in Example 3. After the repair, the repaired parts of the reinforced concrete blocks were subjected to compressive strength, frost resistance, ultraviolet aging tests, bonding, and salt spray tests. The results are shown in Table 3 below:

[0091] Table 3

[0092]

[0093] By comparison of Examples 3, 6, and 7, it can be seen that during the carbonization oxidation process, the compressive strength gradually increases with the increase of carbonization time, indicating that within a certain range, the compressive strength of the cementitious material increases with the increase of carbonization time.

[0094] Similarly, regarding the test of carbonization pressure under carbonization conditions, the compressive strength gradually increases with the increase of carbonization pressure during the carbonization oxidation process. Within a certain range, the compressive strength of cementitious materials increases with the increase of carbonization pressure at any time.

[0095] In combination with Examples 3, 4, 5, 6, 7 and the carbonization pressure, it can be further said that within the allowable range, the higher the carbonization time, the content of carbon dioxide in the curing gas, and the carbonization pressure, the better the carbonization degree, the denser the structure, and the higher the compressive strength; however, after the carbonization reaches a certain degree (saturation, near saturation, qualified degree of detection), a carbonization time that is too long may easily cause a waste of curing gas, increase costs, etc.; the same applies to carbonization pressure and carbonization time.

[0096] Comparative Example 1:

[0097] The difference between Comparative Example 1 and Examples 1 to 3 is that conventional repair and maintenance methods of the prior art (not the carbonization maintenance involved in this application) are adopted.

[0098] In Examples 1 to 3 and Comparative Example 1, similar damaged grooves of 100mmX100mmX80mm reinforced concrete blocks were repaired under the same conditions. After the repair, the repaired parts of the reinforced concrete blocks were subjected to compressive strength, frost resistance, ultraviolet aging tests, bonding, and salt spray tests. The results are shown in Table 4 below:

[0099] Table 4: Experimental results of Examples 1 to 3 and Comparative Example 1

[0100]

[0101]

[0102] According to the test results, the compressive strength, frost resistance, tolerance to ultraviolet rays, degree of bonding between the repair material and the repaired part, and salt spray test results of Examples 1 to 3 are all better than those of Comparative Example 1. This is because the structure of the cementitious material in the repair material is more dense and stable after carbonization, which effectively illustrates that the repair material provided by the present application has good compressive strength and frost resistance, strong tolerance to ultraviolet rays, and good bonding and corrosion resistance.

[0103] Comparative Example 2:

[0104] In Examples 1 to 3, Comparative Examples 1 and 2, similar damaged grooves of reinforced concrete blocks of 100mmX100mmX80mm were repaired under the same conditions;

[0105] The difference between Comparative Example 2 and Examples 1 to 3 is that no rock wool particles and filamentary rock wool are added in Comparative Example 2;

[0106] The compressive strength tests of Examples 1 to 3, Comparative Example 1 and Comparative Example 2 were performed for 1 h, 24 h and 48 h, respectively. The specific test results are shown in Table 5:

[0107] Table 5: Compressive strength test results of Examples 1 to 3, Comparative Example 1 and Comparative Example 2

[0108]

[0109] According to the test results, compared with Examples 1 to 3, the compressive strength of Comparative Example 2 is lower than that of Examples 1 to 3. This is because Comparative Example 2 does not add rock wool particles that play a skeleton support role and filamentous rock wool that plays a toughening role, resulting in poor compressive strength;

[0110] Compared with Comparative Example 1, the compressive strength of Comparative Example 2 is higher than that of Comparative Example 1. This is because the cementitious material in the repair material of the reinforced concrete structure provided by Comparative Example 2 effectively improves its compressive strength after carbonization; it further illustrates that the addition of rock wool particles and filamentary rock wool can not only effectively utilize the waste rock wool, but also have an enhancing effect, thereby achieving the goal of high-value waste utilization.

[0111] Comparative Example 3:

[0112] The difference from Example 2 is that in Comparative Example 3, only 20 parts of rock wool particles are added;

[0113] Comparative Example 4:

[0114] The difference from Example 2 is that in Comparative Example 4, only 20 parts of filamentous rock wool are added;

[0115] For Example 2, Comparative Example 3 and Comparative Example 4, similar damaged grooves of 100mmX100mmX80mm reinforced concrete blocks were repaired under the same conditions, and the compressive strength tests were carried out for 1h, 24h and 48h. The specific test results are shown in Table 6:

[0116] Table 6

[0117]

[0118] According to the test results, compared with Example 2, the compressive strength of Comparative Examples 3 and 4 is lower than that of Example 2, and the compressive strength of Comparative Example 3 is slightly higher than that of Comparative Example 4. The rock wool particles play a skeleton support role and the filamentous rock wool plays a toughening role, which can promote the improvement of compressive strength.

[0119] Embodiment 8:

[0120] The difference between Example 8 and Examples 1 to 3 is that 1 part of ceramic slag and 1 part of shell slag are added in Example 8;

[0121] Example 9

[0122] The difference between Example 9 and Examples 1 to 3 is that 2 parts of ceramic slag and 2 parts of shell slag are added in Example 9;

[0123] Example 10

[0124] The difference between Example 10 and Examples 1 to 3 is that 3 parts of ceramic slag and 3 parts of shell slag are added in Example 10;

[0125] In Examples 1 to 3 and Examples 8 to 10, similar damaged grooves of reinforced concrete blocks of 200 mm x 200 mm x 150 mm were repaired under the same conditions.

[0126] The water penetration resistance test was performed on Examples 1 to 3 and Examples 8 to 10 respectively. The water pressure applied by the water permeation tester was in the range of 0.1 to 2.0 MPa. The specific test results are shown in Table 6:

[0127] Table 7: Test results of water penetration resistance of Examples 1 to 3 and Examples 8 to 10

[0128]

[0129]

[0130] According to the test results, compared with Examples 1 to 3, the water penetration resistance of Examples 8-10 is similar to or better than that of Examples 1 to 3. This is because hydrophobic ceramic slag and shell slag are added to Examples 8-10, and the combination of the two with the cementitious material improves the waterproof performance.

[0131] Compared with Comparative Example 1, Examples 8-10 have higher wear resistance and waterproof properties than Comparative Example 1. This is because the cementitious material and ceramic slag and shell residue in the repair material of the reinforced concrete structure provided by Examples 8-10 have a synergistic effect; it further illustrates that adding ceramic slag and shell residue is feasible, not only can the discarded ceramic slag and shell residue be effectively utilized, but also can have a waterproof effect, and as the amount of ceramic slag and shell residue added increases, the waterproof performance is gradually improved.

[0132] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A repair material for reinforced concrete structure, characterized in that: The raw materials include the following by weight: 90-110 parts of cementitious materials, 15-25 parts of rock wool, 0.01-0.1 parts of defoaming agents, 18-24 parts of water; 1-3 parts by weight of ceramic slag, 1-3 parts by weight of shell slag; the cementitious materials include calcium silicate or calcium-based and magnesium-based industrial solid waste; the calcium silicate includes one or more of γ-type dicalcium silicate, β-type dicalcium silicate, monocalcium silicate, dicalcium silicate, tricalcium silicate, calcium oxide or calcium hydroxide; the calcium-based and magnesium-based industrial solid waste includes one or more of steel slag, magnesium slag, carbide slag, phosphogypsum, and waste rock powder; The rock wool is rock wool particles and filamentary rock wool; the rock wool particles are obtained by granulating waste rock wool or waste building materials; the particle size of the rock wool particles is 0.5mm-80mm; the filamentary rock wool is obtained by crushing, loosening and combing waste rock wool; a water repellent is sprayed on the filamentary rock wool; the concentration of the water repellent is 35%-45% methyl silicate solution.

2. The repair material according to claim 1, characterized in that: The defoamer is selected from any one of a high-carbon alcohol defoamer or a polyether defoamer; the high-carbon alcohol defoamer includes one or more of a silicone defoamer, a polyester defoamer, a n-butanol defoamer or a fatty alcohol defoamer; the polyether defoamer includes one or more of a GP-type glycerol polyether, a GPE-type polyoxyethylene polyoxypropylene glycerol ether or a silicone-polyether composite defoamer.

3. A method for preparing a repair material for a reinforced concrete structure according to any one of claims 1 to 2, characterized in that: The steps include: A) mixing the cementitious material and the rock wool particles to obtain a mixed dry material; B) The filamentous rock wool, water and mixed dry materials are mixed and stirred uniformly, and a defoaming agent is added to obtain the product.

4. A method for using a repair material for a reinforced concrete structure, characterized in that: include: Use the repair material for reinforced concrete structure as claimed in any one of claims 1 to 2 to fill and fill cracks or damages in the reinforced concrete structure; Then carbonization curing is carried out.

5. The method of use according to claim 4, characterized in that: The carbonization curing conditions are as follows: carbonization gas: industrial waste gas with a carbon dioxide content of not less than 1%; carbonization temperature of 0 to 45° C., carbonization pressure of 0 to 1 MPa, and carbonization time of 1 to 72 hours.

6. Use of a repair material for reinforced concrete structures as claimed in any one of claims 1 to 2 or a repair material prepared by the preparation method as claimed in claim 3 in treating cracks in reinforced concrete structures, corner chips in concrete, surface damage in concrete, indentations in concrete, collapse in concrete or cracks in concrete.