A method for pretreatment of hydrogen

Through the multi-level catalyst bed and gradient design of the H2-TPR hydrogen consumption peak temperature, combined with the use of inorganic or organic additives, the interaction between the catalyst activity and the carrier is optimized, solving the problem of mismatching the molecular structure of the catalyst and the reactant, and improving It improves the depth and stability of the hydrogenation reaction and achieves more efficient desulfurization and denitrification effects.

CN116023986BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111242765.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-25
Publication Date
2024-10-01
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

In existing hydrocracking technology, the catalyst grading method fails to effectively consider the relationship between the catalyst active phase properties and reaction conditions, resulting in limited depth of hydrodesulfurization and denitrification reactions. Especially in the process of heavy oil treatment, the catalyst and The molecular structure of the reactants does not match, which affects the depth of the reaction.

Method used

Using a multi-level hydrotreating catalyst bed structure, through the gradient design of H2-TPR hydrogen consumption peak temperature and average reaction temperature, combined with the use of different inorganic or organic additives, the heat treatment conditions of the catalyst are adjusted, and the active metal and active metal of the catalyst are optimized. The carrier interacts to improve the coupling performance between the active center of the catalyst and the molecular structure of the reactant.

Benefits of technology

It significantly improves the overall desulfurization and denitrogenation performance of the hydrogenation reactor, is suitable for the hydrogenation of various distillate oils, improves the stability and depth of the reaction, and improves the quality of the oil produced by hydrorefining.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a hydrogenation pretreatment method, wherein N hydroprocessing catalyst beds are arranged along the flow direction of the logistics, wherein N is an integer greater than 2, preferably an integer greater than 3, more preferably N is 3 to 5, and more preferably N is 3, and the hydroprocessing catalyst H loaded in the first hydroprocessing catalyst bed is 2 The peak temperature of hydrogen consumption in TPR (℃) is higher than that of the hydroprocessing catalyst H loaded in the Nth hydroprocessing catalyst bed. 2 The method can improve the overall desulfurization and denitrification performance of the hydroprocessing reactor and can be applied to the hydroprocessing process of various distillate oils.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hydrogenation pretreatment method, in particular to a hydrogenation treatment method with deep denitrification and high hydrogenation saturation performance. Background Art

[0002] In modern oil refining technology, hydrocracking refers to those hydrogenation processes that convert more than 10% of macromolecular compounds in the raw materials into small molecular compounds through hydrogenation reactions. It has the characteristics of strong raw material adaptability, large production plan flexibility, and good product quality. Therefore, it has become one of the important process technologies for deep processing of heavy oil. The core of hydrocracking technology is the catalyst, including pretreatment catalyst and cracking catalyst. Among them, the main function of the hydrocracking pretreatment catalyst is to hydrogenate and remove impurities such as sulfur, nitrogen, oxygen and heavy metals contained in the raw materials, as well as hydrogenate saturated polycyclic aromatic hydrocarbons to improve the properties of the oil. Because the nitrides in the raw oil, especially the alkaline nitrides, can poison the acid center of the cracking catalyst, the hydrodenitrogenation performance is an important indicator for measuring the hydrocracking pretreatment catalyst.

[0003] The reactions in the heavy oil hydroprocessing process mainly include hydrodesulfurization, hydrodenitrogenation, hydrodemetallization, aromatic saturation and hydrocracking of various hydrocarbons. When the heavy raw materials enter the reactor, the molecular structure of the reactants is complex, the steric hindrance is large, and the impurities are easier to remove; with the hydrogenation and hydrogenolysis reactions, the reactant molecules gradually open the ring and break the chain, the molecular structure is gradually simplified, the steric hindrance is small, and the impurities are more difficult to remove. At present, the grading method of heavy oil hydrogenation catalyst is often studied from the surface level, that is, the catalyst particle size, pore size and activity transition, and the actual reactant molecular structure level is not considered. As the reaction proceeds, the reactant molecular structure and the catalyst structure cannot match well, which limits the depth of the hydrogenation reaction.

[0004] CN109593554A relates to a catalyst for hydrotreating coal tar, and specifically to a catalyst grading method for hydrotreating coal tar. It is composed of a hydrogenation protection catalyst-hydrogenation demetallization catalyst-mild hydrorefining catalyst-mild hydrocracking catalyst-deep hydrorefining catalyst. The device of the present invention is three fixed bed refining reactors arranged in series, wherein the hydrogenation protection catalyst and the hydrodemetallization catalyst are respectively loaded into the upper bed layer and the lower bed layer of the first reactor; the mild hydrorefining catalyst is respectively loaded into the three beds of the second reactor; the mild hydrocracking catalyst is loaded into the upper bed layer of the third reactor; and the deep hydrorefining catalyst is loaded into the middle and lower beds of the third reactor. The catalyst grading method of the present invention is used to hydrorefining the pretreated coal tar on a fixed bed hydrogenation device, and the produced hydrorefining oil can be used as a feedstock oil for producing high-density aviation kerosene and low-freezing point diesel.

[0005] CN111073689A discloses a heavy oil hydrogenation treatment method, including the following contents: the heavy oil raw material enters the hydrogenation reactor, contacts with the hydrogenation catalyst bed layer for hydrogenation reaction, and the reaction product flows out of the reactor; wherein the hydrogenation catalyst bed layer is graded and loaded with at least two levels of sulfurized hydrogenation catalyst along the logistics direction, and the average length of the metal active phase lamellae increases step by step, the average number of lamellae decreases step by step, the content of active components increases step by step, and the aperture decreases step by step along the logistics direction. The method of the present invention adopts a specific catalyst gradation to effectively utilize the catalyst active center, improve the coupling reaction performance of the active center structure and the reactant molecular structure, greatly improve the stability of the hydrogenation reaction of the entire system, such as demetallization, desulfurization, denitrogenation, etc., and is conducive to the deep hydrogenation of heavy oil.

[0006] The existing technologies mostly study the grading of catalyst activity and catalyst particle size, without considering the influence of the correlation between the properties of the catalyst active phase and the reaction conditions. In particular, for hydrodesulfurization and hydrodenitrogenation reactions, the surface properties of the catalyst have an important influence. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides a grading method for a hydroprocessing catalyst, which is applicable to the hydroprocessing process of various distillate oils. The method can improve the overall desulfurization and denitrification performance of the hydroprocessing reactor and can be applicable to the hydroprocessing process of various distillate oils.

[0008] A hydroprocessing method, wherein N hydroprocessing catalyst beds are arranged along a flow direction of a logistics stream, wherein N is an integer greater than 2, preferably an integer greater than 3, more preferably N is 3 to 5, and even more preferably N is 3, and the peak temperature (°C) of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the first hydroprocessing catalyst bed is higher than the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the Nth hydroprocessing catalyst bed.

[0009] In the method of the present invention, the peak temperature (°C) of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the first hydroprocessing catalyst bed is higher than the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the Nth hydroprocessing catalyst bed, generally 10°C-200°C, preferably 10°C-100°C, and further preferably 10°C-60°C.

[0010] In the method of the present invention, the average reaction temperature of the Nth hydroprocessing catalyst bed is higher than the average reaction temperature of the N-1th hydroprocessing catalyst bed.

[0011] In the method of the present invention, the average reaction temperature of the Nth hydroprocessing catalyst bed is generally 5°C-50°C higher than the average reaction temperature of the N-1th hydroprocessing catalyst bed, preferably 5°C-40°C, and more preferably 10°C-30°C.

[0012] In the method of the present invention, when N is an integer greater than 3, the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the N-1th hydroprocessing catalyst bed is higher than or equal to the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the N-2th hydroprocessing catalyst bed, and the higher temperature is generally 5°C-60°C, preferably 10°C-50°C.

[0013] In the method of the present invention, the packing volume ratio of adjacent catalyst beds is 1:20 to 20:1, preferably 1:10 to 10:1, and more preferably 1:5 to 5:1.

[0014] In the method of the present invention, the hydroprocessing catalyst with different peak temperatures of H2-TPR hydrogen consumption can be commercially available or prepared by any existing catalyst adjustment technology. For example, different inorganic or organic additives are introduced during the preparation of the carrier and the catalyst, and the heat treatment temperature of the catalyst is changed. Taking the introduction of different inorganic or organic additives during the preparation of the carrier and the catalyst as an example, the inorganic additive is one or more of fluorine, silicon, phosphorus, boron, magnesium, zirconium, etc. The organic additive is one or more of nitrogen-containing organic compounds, sulfur-containing organic compounds and oxygen-containing organic compounds. The inorganic or organic additive can be introduced in any step, such as before, at the same time and after the impregnation of the Group VIB and Group VIII metal components. The nitrogen-containing organic compound is an organic substance containing at least one covalently bonded nitrogen atom, such as ethanolamine, diethanolamine, triethanolamine, ethylenediaminetetraacetic acid (EDTA), nitrilotriacetic acid (NTA) and ethylenediaminetetraacetic acid. The sulfur-containing organic compound is an organic substance containing at least one covalently bonded sulfur atom, such as mercaptan (general formula R-SH), thioether (general formula R-S-R), disulfide (general formula R-S-S-R), and R in these sulfur-containing compounds is an alkyl group containing 1 to 10 carbon atoms, such as ethyl mercaptan, ethylpropyl sulfide, dimethyl disulfide, etc. The sulfur-containing organic compound may contain one or more carboxyl, carbonyl, ester, ether, hydroxyl, and thiol group substitutions, such as thioglycolic acid, thiopropionic acid, dimercaptopropanol, etc. In addition to the above-mentioned sulfur-containing compounds, sulfone and sulfoxide compounds may be included, such as dimethyl sulfoxide, dimethyl sulfone, etc. The oxygen-containing organic compound is an organic substance containing at least one carbon atom and one oxygen atom. The oxygen-containing part may be a carboxyl, carbonyl, hydroxyl part, or a combination thereof. These substances can be acids, such as acetic acid, oxalic acid, malonic acid, tartaric acid, malic acid, citric acid, etc., alcohols, such as ethylene glycol, propylene glycol, butylene glycol, glycerol, trimethylolethane, etc., ethers, such as diethylene glycol, dipropylene glycol, triethylene glycol, tributylene glycol, tetraethylene glycol, polyethylene glycol, etc., sugars, such as glucose, fructose, lactose, maltose, sucrose, etc., and ketones, phenols, aldehydes and lipids. Different drying and / or calcination heat treatment temperatures also have an important influence on the surface nickel atom concentration of the hydroprocessing catalyst. When treated at low temperature, the surface nickel atom concentration of the hydroprocessing catalyst with the same nickel element mass content is higher; when treated at high temperature, the surface nickel atom concentration of the hydroprocessing catalyst with the same nickel element mass content is lower. The low temperature and high temperature are relative, and the treatment temperature range is 80°C~800°C. For example, you can customize the heat treatment temperature of 80°C~300°C, preferably 120°C~200°C as low temperature treatment; the heat treatment temperature of 350°C~800°C, preferably 400°C~600°C is considered as high temperature treatment.

[0015] In the method of the present invention, the H2-TPR method is used to determine the strength of the interaction between the active metal of the catalyst and the carrier. The lower the peak temperature of the H2-TPR hydrogen consumption, the weaker the interaction force. The peak temperature range is between 230°C and 480°C, preferably 280°C to 450°C.

[0016] In the method of the present invention, the method can process a variety of distillate oil raw materials, including various diesel, VGO, CGO, DAO and mixed oils of two or more thereof, and its main properties are as follows: distillation range, initial distillation point greater than 180°C, final distillation point less than 600°C; density, 0.8000~0.9500 / g·cm -3 (20℃); Nitrogen content, 100~6000μg·g -1 ; Sulfur content, 0.05%~3.0%.

[0017] In the method of the present invention, the hydroprocessing catalyst contains group VIB and group VIII metal components. The active metal of group VIB is W and / or Mo, and the active metal of group VIII is Ni and / or Co. The active metals in the final hydroprocessing catalyst are generally 9% to 50% of group VIB metal oxides and 1% to 15% of group VIII metal oxides by weight of oxides. The catalyst carrier is a porous refractory oxide, such as alumina, silica, silica-alumina, alumina in which silica-alumina is dispersed, alumina coated with silica, magnesium oxide, zirconium oxide, boron oxide, titanium dioxide, etc. According to the use requirements of the catalyst, suitable additives can be added, such as one or more of fluorine, phosphorus, boron, magnesium, zirconium, etc.

[0018] In the method of the present invention, the reaction conditions are as follows: the reaction pressure is 3MPa~20MPa, preferably 8MPa~17MPa, and the air velocity is 0.2h -1 ~4.0h -1 , preferably 0.8h -1 ~2.0h -1 The reaction temperature is 260°C~430°C, preferably 300°C~400°C.

[0019] When the method of the present invention is adopted, when the metal carrier interacts strongly, the obtained active phase has a strong ability to dissociate hydrogen, and the reaction effect is good at low temperature; when the metal carrier interacts weakly, the active phase has a strong ability to transfer hydrogen, and the reaction effect is good at high temperature. The temperature in the direction of the reactor logistics gradually rises, and this catalyst graded loading method is conducive to improving the overall desulfurization and denitrification effect of the device. DETAILED DESCRIPTION

[0020] H2-TPR characterization was performed using a fully automatic chemisorption instrument (AMI-200) from Altamira, USA. The carrier gas was high-purity argon, and the sample was pretreated at 485°C for 1 h before the measurement. Then 5% H2-Ar was used as the reaction gas and the temperature was programmed to 700°C at a heating rate of 10°C / min.

[0021] The detailed process of the present invention is further described below by way of examples, but the present invention should not be considered to be limited to these examples. Unless otherwise specified, % in the following examples and comparative examples are all mass percentages. The pore structure of the alumina carrier used in the examples and comparative examples is shown in Table 1:

[0022] Table 1 Properties of carriers used in the examples and comparative examples

[0023]

[0024] Example 1

[0025] This example provides the preparation method of the catalyst used in the examples and comparative examples, but the following preparation method is not the only one and does not constitute a limitation to the present invention.

[0026] Preparation method of catalyst CAT1: The alumina carrier S1 is impregnated with equal volumes of impregnation solutions containing Mo and Ni, dried at 120°C for 3 hours, and calcined at 550°C for 2 hours. The obtained catalyst is recorded as CAT1.

[0027] Preparation method of catalyst CAT2: The alumina carrier S2 is impregnated with equal volumes of impregnation solution containing Mo and Ni, dried at 120°C for 3 hours, and calcined at 450°C for 2 hours. The obtained catalyst is recorded as CAT2.

[0028] Preparation method of catalyst CAT3: impregnate alumina carrier S2 with equal volumes of impregnation solution containing Mo and Ni, the impregnation solution contains citric acid, the molar ratio of citric acid to nickel atoms is 0.4:1, and dry at 120°C for 3h. The obtained catalyst is recorded as CAT3.

[0029] Table 2 Main properties of the prepared oxidized catalysts

[0030]

[0031] Example 2

[0032] This example provides a loading scheme for evaluating the catalyst. Three reaction beds are set along the direction of the reactant flow, with bed volumes of 25 mL, 25 mL and 50 mL, respectively, and the reaction temperatures are controlled at 330°C, 350°C and 380°C, respectively.

[0033] The test number is PS1: the three reaction beds are sequentially loaded with catalyst CAT1, catalyst CAT2 and catalyst CAT3 along the direction of reactant flow.

[0034] The test number is PS2: the three reaction beds are sequentially loaded with catalyst CAT1, catalyst CAT1 and catalyst CAT3 along the direction of reactant flow.

[0035] The test number is PS3: the three reaction beds are sequentially loaded with catalyst CAT2, catalyst CAT2 and catalyst CAT3 along the direction of reactant flow.

[0036] Comparative Example 1

[0037] This comparative example provides a loading scheme for evaluating the catalyst. Three reaction beds are set along the direction of the reactant flow, with bed volumes of 25 mL, 25 mL and 50 mL, respectively, and the reaction temperatures are controlled at 330°C, 350°C and 380°C, respectively.

[0038] The test number is PD1: along the direction of the reactant flow, the three reaction beds are sequentially loaded with catalyst CAT3, catalyst CAT2 and catalyst CAT1.

[0039] The test number is PD2: along the direction of the reactant flow, the three reaction beds are sequentially loaded with catalyst CAT2, catalyst CAT2 and catalyst CAT2.

[0040] The test number is PD3: along the direction of the reactant flow, the three reaction beds are sequentially loaded with catalyst CAT3, catalyst CAT3 and catalyst CAT3.

[0041] Example 3

[0042] This example is an activity evaluation experiment of the catalyst.

[0043] The catalyst activity evaluation experiment was carried out on a three-tube series small hydrogenation unit. The catalyst was presulfurized before the activity evaluation. The catalyst evaluation conditions were a total reaction pressure of 14.7 MPa and a liquid hourly space velocity of 1.0 h -1 , hydrogen-to-oil volume ratio 900:1, the properties of the raw oil used in the activity evaluation experiment are shown in Table 3, and the activity evaluation results are shown in Table 4.

[0044] Table 3 Raw oil properties

[0045]

[0046] Table 4400 hours catalyst activity evaluation results

[0047]

[0048] It can be seen from the evaluation results in Table 4 that, compared with the comparative example, the denitrification and desulfurization activities of the catalyst system are greatly improved by using the loading method of the hydroprocessing catalyst of the present invention, and high-quality feed can be provided for subsequent devices.

Claims

1. A method for desulfurization and denitrification by hydrotreatment, characterized in that: The method sets N hydroprocessing catalyst beds along the flow direction of the logistics, wherein N is an integer greater than 2, and the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the first hydroprocessing catalyst bed is 10°C-200°C higher than the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the Nth hydroprocessing catalyst bed; The average reaction temperature of the Nth hydroprocessing catalyst bed is 5°C-50°C higher than the average reaction temperature of the N-1th hydroprocessing catalyst bed; The hydroprocessing catalyst contains Group VIB and Group VIII metal components, wherein the Group VIB metal is W and / or Mo, and the Group VIII metal is Ni and / or Co; the active metals in the final hydroprocessing catalyst are calculated by weight of oxides: the content of Group VIB metal oxides is 9%-50%, and the content of Group VIII metal oxides is 1%-15%.

2. The method according to claim 1, characterized in that: The N is an integer greater than or equal to 3.

3. The method according to claim 1, characterized in that: The N is 3 to 5.

4. The method according to claim 1, characterized in that: The N is 3.

5. The method according to claim 1, characterized in that: The peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the first hydroprocessing catalyst bed is 10°C-100°C higher than the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the Nth hydroprocessing catalyst bed.

6. The method according to claim 1, characterized in that: The peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the first hydroprocessing catalyst bed is 10° C.-60° C. higher than the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the Nth hydroprocessing catalyst bed.

7. The method according to claim 1, characterized in that: The average reaction temperature of the Nth hydroprocessing catalyst bed is 5° C. to 40° C. higher than the average reaction temperature of the N-1th hydroprocessing catalyst bed.

8. The method according to claim 7, characterized in that: The average reaction temperature of the Nth hydroprocessing catalyst bed is 10° C. to 30° C. higher than the average reaction temperature of the N-1th hydroprocessing catalyst bed.

9. The method according to claim 1, characterized in that: When N is an integer greater than 3, the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the N-1th hydroprocessing catalyst bed is equal to the peak temperature of hydrogen consumption of the hydroprocessing catalyst H2-TPR loaded in the N-2th hydroprocessing catalyst bed.

10. The method according to claim 1, characterized in that: The packing volume ratio of adjacent catalyst beds is 1:20~20:

1.

11. The method according to claim 10, characterized in that: The packing volume ratio of adjacent catalyst beds is 1:10~10:

1.

12. The method according to claim 10, characterized in that: The packing volume ratio of adjacent catalyst beds is 1:5~5:

1.

13. The method according to claim 1, characterized in that: The properties of the crude oil are as follows: distillation range, initial distillation point greater than 180°C, final distillation point less than 600°C; density at 20°C 0.8000~0.9500 / g·cm -3 ; Nitrogen content 100~6000μg·g -1 ; Sulfur content 0.05wt%~3.0wt%.

14. The method according to claim 1, characterized in that: The reaction conditions of the hydrotreatment are as follows: the reaction pressure is 3MPa~20MPa, the liquid hourly volume space velocity is 0.2h -1 ~4.0h -1 , the reaction temperature is 260℃~430℃.

15. The method according to claim 14, characterized in that: The reaction conditions of the hydrotreatment are as follows: the reaction pressure is 8MPa~17MPa, the liquid hourly volume space velocity is 0.8h -1 ~2.0h -1 , the reaction temperature is 300℃~400℃.