A beryllium-tungsten alloy with high temperature, high toughness and high neutron multiplication rate and its application
By adjusting the composition and structure of beryllium-tungsten alloy, the problem of radiation swelling and neutron reproduction performance of beryllium materials in high-temperature and high-irradiation environments was solved, and a beryllium-tungsten alloy with high temperature, high toughness and high neutron reproduction rate was developed to achieve excellent radiation resistance. It has excellent photo-swelling and neutron breeding properties and is suitable for nuclear fusion reactors and high-temperature materials.
Patent Information
- Application Number
- CN202211648540.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-21
AI Technical Summary
Existing beryllium materials swell significantly under high-temperature and high-irradiation environments, which affects the safe operation of nuclear fusion reactors. In addition, beryllium-titanium alloys have reduced neutron reproduction performance and poor toughness, making it difficult to meet the needs of future commercial fusion reactors.
Develop a beryllium-tungsten alloy with high temperature, high toughness and high neutron reproduction rate. Its composition is Bea(WbMc)Xd, where M is Re, Zr, Y, Mg, Ti, V, Mn, Fe, Co, Cr, W, Mo ,Nb,Pb,Bi,Ta ,Hf,Tl, Improve neutron proliferation rate and radiation swelling resistance.
It achieves an excellent combination of high-temperature properties, mechanical properties and neutron breeding properties of beryllium-tungsten alloy. It has a wide range of preparation conditions and excellent radiation swelling resistance, and is suitable for the field of neutron breeding and high-temperature materials.
Smart Images

Figure CN116024473B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials, and in particular relates to a beryllium-tungsten alloy with high temperature, high toughness and high neutron multiplication rate and its application. Background Art
[0002] Nuclear fusion energy, as an internationally recognized clean energy, is gradually coming into people's view. In nuclear fusion reactors, neutron breeders are an important factor in achieving the self-sustaining of fusion fuel tritium and even the ultimate commercial application of fusion energy.
[0003] Beryllium is an excellent neutron breeding material. The binding energy of beryllium neutrons in the nucleus is small (1.666MeV), which is equivalent to 1 / 5 to 1 / 6 of the energy of most stable atoms. Neutrons are easily released through bombardment of high-energy particles, including (n,2n) reactions, thereby achieving neutron proliferation. Metallic beryllium has no obvious irradiation swelling (<3%) below 400°C and transmutation He injection below 3000appm, and has been selected as the neutron breeder in the blanket of the ITER nuclear fusion reactor. However, the future commercial controlled fusion reactor (DEMO) will have a more harsh environment, higher operating temperature (600-900°C), greater irradiation dose, and helium injection of up to 20,000appm. The irradiation swelling of beryllium is particularly obvious (>3%), which may endanger the operation of the reactor.
[0004] Beryllium intermetallic compounds, such as Be 12 Ti has attracted the attention of researchers, and foreign countries, especially Japan, have paid attention to Be 12 Ti has been extensively studied. However, due to the addition of Ti, Be 12 The neutron multiplication performance of Ti is greatly reduced, and the toughness is very poor, which is extremely unfavorable for the production and use of beryllium-titanium alloys and neutron multiplier pellets. Tungsten has the advantages of high melting point, low activation, and the ability to form high-temperature resistant intermetallic compounds with beryllium, but it also has disadvantages such as poor toughness and poor processing performance. Therefore, the study of new beryllium-tungsten alloys with higher toughness and higher neutron multiplication performance is of great significance in the field of fusion neutron multiplication and even in the high-temperature field. Summary of the invention
[0005] In order to overcome the above problems existing in the prior art, the present invention provides a beryllium tungsten alloy with high temperature, high toughness and high neutron multiplication rate and its application, which are used to solve the above problems existing in the prior art.
[0006] A beryllium tungsten alloy with high temperature, high toughness and high neutron multiplication rate, characterized in that the atomic percentage expression of the beryllium tungsten alloy material composition is Be a (W b M c )X d, where M is one or more of Re, Zr, Y, Mg, Ti, V, Mn, Fe, Co, Cr, W, Mo, Nb, Pb, Bi, Ta, Hf, Tl, X is one or more of O, C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, 63 ≤ a ≤ 97, 3 ≤ b ≤ 37, 0 ≤ c ≤ 37, 0 ≤ d ≤ 3, and a + b + c + d = 100.
[0007] For the aspects and any possible implementation manners as described above, a further implementation manner is provided. When 0 < d ≤ 2, 0 ≤ c ≤ 2.17, c < b ≤ 4.35, 93.65 ≤ a ≤ 97, the beryllium tungsten alloy includes a face-centered cubic structure phase and a hexagonal close-packed structure phase, and the grain size ≤ 80 μm.
[0008] For the aspects and any possible implementation manners as described above, a further implementation manner is provided. When d = 0, 0 < c ≤ 2.17, 0 < c < b ≤ 4.35, a = 95.65, the atomic percentage expression of the beryllium tungsten alloy material composition is Be 95.65 (W,M) 4.35 , and the beryllium tungsten alloy is of a face-centered cubic structure, and the grain size ≤ 80 μm.
[0009] For the aspects and any possible implementation manners as described above, a further implementation manner is provided. When d = 0, 2 < c ≤ 3.84, c < b ≤ 7.69, a = 92.31, the atomic ratio expression of the beryllium tungsten alloy material composition is Be 92.31 (W,M) 7.69 , and the beryllium tungsten alloy includes a tetragonal structure and a face-centered cubic structure, and the grain size ≤ 80 μm.
[0010] For the aspects and any possible implementation manners as described above, a further implementation manner is provided. When 0 < d ≤ 2, 0 < c ≤ 3.84, c < b ≤ 7.69, 90.31 < a < 95.65, the beryllium tungsten alloy includes a face-centered cubic phase and a tetragonal structure phase, and the grain size ≤ 80 μm.
[0011] For the aspects and any possible implementation manners as described above, a further implementation manner is provided. When 0 < d ≤ 2, 0 < c ≤ 18.5, c < b ≤ 37, 61 ≤ a < 92.31, the beryllium tungsten alloy includes a tetragonal structure phase and a hexagonal structure phase, and the grain size ≤ 80 μm.
[0012] For the aspects and any possible implementation manners as described above, a further implementation manner is provided. When d = 1.98, c = 1.75, b = 7.41, a = 88.86, the atomic percentage expression of the beryllium tungsten alloy material composition is Be 88.86 W 7.41 M 1.75X 1.98 , including tetragonal structure phase and hexagonal structure phase, with grain size ≤80um.
[0013] According to the above aspects and any possible implementation, an implementation is further provided, wherein the melting point of the beryllium tungsten alloy is about 2200° C., and the neutron multiplication rate is about 0.96.
[0014] According to the above aspects and any possible implementation, a further implementation is provided. When d=1.98, c=1.75, b=4.19, a=92.08, the atomic percentage expression of the beryllium tungsten alloy material composition is Be 92.08 W 4.19 M 1.75 X 1.98 , it has a face-centered cubic structure and the grain size is ≤80um.
[0015] According to the above aspects and any possible implementation, a further implementation is provided, when d=1.98, c=1.75, b=2.51, a=93.76, the atomic percentage expression of the composition of the beryllium tungsten alloy material is Be 93.76 W 2.51 M 1.75 X 1.98 , it has a face-centered cubic structure and the grain size is ≤80um.
[0016] The present invention also provides an application of a high-temperature, high-toughness, and high-neutron multiplication rate beryllium-tungsten alloy in a neutron multiplier for a fusion reactor.
[0017] Beneficial effects of the present invention
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The beryllium tungsten alloy with high temperature, high toughness and high neutron proliferation rate of the present invention has the atomic percentage expression of Be a (W b M c )X d , which has the following advantages:
[0020] 1. Beryllium tungsten alloy has a large composition range and a wide range of preparation conditions.
[0021] 2. By adjusting the alloy composition, heat treatment, hot and cold processing technology, etc., controlling the phase composition and refining the grains, different high-temperature properties, mechanical properties and neutron multiplication properties can be obtained.
[0022] 3. The main elements of the high-temperature, high-toughness, and high-neutron proliferation rate beryllium-tungsten alloy material provided by the present invention are common metal raw materials and compounds, and can be prepared by different preparation methods, with the advantages of convenient preparation, simple process, and economy.
[0023] 4. The beryllium tungsten alloy prepared by the present invention has excellent high-temperature performance, a melting point of about 2200°C, a neutron multiplication rate of about 0.96, and excellent anti-irradiation swelling performance and mechanical properties.
[0024] 5. The beryllium tungsten alloy provided by the present invention has excellent mechanical properties, high temperature properties, excellent anti-irradiation swelling properties and neutron proliferation properties, and can be widely used in the fields of neutron proliferation, plasma-oriented materials and high temperature materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM image of the phase composition of the beryllium tungsten alloy of Example 1 of the present invention. DETAILED DESCRIPTION
[0026] In order to better understand the technical solution of the present invention, the content of the present invention includes but is not limited to the specific implementation methods described below, and similar technologies and methods should be considered to be within the scope of protection of the present invention. In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments.
[0027] It should be clear that the embodiments described in the present invention are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0029] The beryllium tungsten alloy with high temperature, high toughness and high neutron proliferation rate of the present invention has the atomic percentage expression of Be a (W b M c )X d, where M is one or more of Re, Zr, Y, Mg, Ti, V, Mn, Fe, Co, Cr, W, Mo, Nb, Pb, Bi, Ta, Hf, Tl, X is one or more of O, C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, 63 ≤ a ≤ 97, 3 ≤ b ≤ 37, 0 ≤ c ≤ 37, 0 ≤ d ≤ 3, and a + b + c + d = 100.
[0030] The beryllium tungsten alloy of the present invention uses doping of neutron multiplication nuclides such as Be, Zr, refractory metal elements with large-sized atoms, and low-activation elements such as W, Re, etc., and auxiliary phases such as Be 95.65 Re 4.35 etc., to obtain a beryllium tungsten alloy with characteristics of high temperature and high neutron multiplication rate, which is applied to neutron multiplication material for fusion reactor, plasma-facing and other structural and functional materials under high temperature environment.
[0031] Furthermore, for the beryllium tungsten alloy with high toughness and high neutron multiplication rate of the present invention, when 0 < d ≤ 2, 0 ≤ c ≤ 2.17, c < b ≤ 4.35, 93.65 ≤ a ≤ 97, the beryllium tungsten alloy is composed of face-centered cubic structure phase and hexagonal close-packed structure phase, the grain size ≤ 80um, and has high toughness and high neutron multiplication performance (>0.96).
[0032] Furthermore, when d = 0, 0 < c ≤ 2.17, 0 < c < b ≤ 4.35, a = 95.65, the atomic percentage expression of the material composition of the beryllium tungsten alloy is Be 95.65 (W,M) 4.35 , the alloy is of face-centered cubic structure, the grain size ≤ 80um, has high neutron multiplication performance (0.96), high toughness, excellent tritium retention performance, and excellent irradiation swelling resistance performance.
[0033] Furthermore, when d = 1.98, c = 1.75, b = 2.51, a = 93.76, the atomic percentage expression of the material composition of the beryllium tungsten alloy is Be 93.76 W 2.51 M 1.75 X 1.98 , the alloy is of face-centered cubic structure, the grain size ≤ 80um, has excellent high-temperature performance, high neutron multiplication rate of 0.96, excellent fracture toughness, tritium retention and irradiation swelling resistance performance.
[0034] When 0 < d ≤ 2, 0 < c ≤ 3.84, c < b ≤ 7.69, 90.31 < a < 95.65, the beryllium tungsten alloy is composed of face-centered cubic and tetragonal structure phases, the grain size ≤ 80um, has a high neutron multiplication rate (>0.92), and excellent tritium retention and irradiation swelling resistance performance.
[0035] Further, when d = 1.98, c = 1.75, b = 4.19, a = 92.08, the atomic percentage expression of the beryllium-tungsten alloy material composition is Be 92.08 W 4.19 M 1.75 X 1.98 , the alloy is a face-centered cubic structure, the grain size ≤ 80um, and has excellent neutron multiplication performance (>0.96), excellent fracture toughness, tritium retention and anti-irradiation swelling performance.
[0036] Further, when d = 0.2 < c ≤ 3.84, c < b ≤ 7.69, a = 92.31, the atomic ratio expression of the beryllium-tungsten alloy material composition is Be 92.31 (W,M) 7.69 , the alloy is composed of a tetragonal structure and a face-centered cubic structure phase, the grain size ≤ 80um, has a high neutron multiplication performance >0.92, and has excellent tritium retention and anti-irradiation swelling performance.
[0037] Further, when 0 < d ≤ 2, 0 < c ≤ 18.5, c < b ≤ 37, 61 ≤ a < 92.31, the beryllium-tungsten alloy is composed of a tetragonal and a hexagonal structure phase, the grain size ≤ 80um, and has excellent high-temperature performance, tritium retention and anti-irradiation swelling performance.
[0038] Further, when d = 1.98, c = 1.75, b = 7.41, a = 88.86, the atomic percentage expression of the beryllium-tungsten alloy material composition is Be 88.86 W 7.41 M 1.75 X 1.98 , the alloy is composed of a tetragonal structure and a hexagonal structure phase, the grain size ≤ 80um, and has excellent high-temperature performance (melting point exceeding 2200 °C), tritium retention and anti-irradiation swelling performance.
[0039] Now describe the method for preparing the beryllium-tungsten alloy of the present invention.
[0040] The preparation method of the beryllium-tungsten alloy of the present invention and the preparation method of the neutron multiplier beryllium-tungsten alloy balls using the same as raw materials adopt hot isostatic pressing method, plasma sintering method, rotating electrode method and powder metallurgy method.
[0041] The preparation of the beryllium-tungsten alloy by the hot isostatic pressing method includes the following steps:
[0042] S1. Weigh pure beryllium powder, titanium powder and other raw materials according to the chemical composition ratio.
[0043] S2. Then mix the proportioned metal powders, and then fill them into a metal cladding (sheath) for high-vacuum sealing and welding, and use the hot isostatic pressing method to press them into an ingot. The manufacturing conditions at this time are as follows:
[0044] Pressure: 100~1000MPa,
[0045] Temperature: 700~1300℃,
[0046] Time: 0.5~6h.
[0047] The plasma sintering method for preparing beryllium tungsten alloy includes the following steps:
[0048] S1. Mix pure beryllium powder, titanium powder and other raw materials according to the chemical composition ratio;
[0049] S2. Then mix the metal powders in the right proportions, and then perform vacuum plasma rapid sintering to form the product. The sintering conditions at this time are described as follows:
[0050] Vacuum degree: 1×10 -1 pa~1×10 -10 Pa
[0051] Temperature: 700~1300℃
[0052] Time: 0.5~6h
[0053] Powder Metallurgy:
[0054] In order to manufacture the neutron multiplier beryllium tungsten alloy microspheres, the neutron multiplier beryllium tungsten alloy is first prepared as a material by the aforementioned method, and then the material is loaded into a mold, crushed, and spheroidized to obtain the microspheres.
[0055] Rotating electrode method:
[0056] The neutron breeder beryllium tungsten alloy microspheres of the present invention are prepared by the rotating electrode method. First, the beryllium tungsten alloy is prepared as the material of the consumable electrode by the aforementioned method. After the material is machined, a specified electrode shape is manufactured to obtain a beryllium tungsten alloy rod of the consumable electrode. Next, the prepared consumable electrode is used to manufacture the neutron breeder beryllium tungsten alloy microspheres by the rotating electrode method. The manufacturing conditions at this time are not particularly limited, and the description of the preferred conditions is as follows:
[0057] Atmosphere gas pressure: 60MPa~1100MPa
[0058] Arc current: 100~1000A
[0059] Consumable electrode rotation speed: 5~1000m / s
[0060] [Example]
[0061] Example 1
[0062] A high temperature and high neutron multiplication rate beryllium tungsten alloy, the composition of which is: Be: 90.93at.%, W: 6.58at.%, O: 0.97at.%, other elements include C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U totaling 1.52at.%, prepared by hot isostatic pressing at a temperature of 1000°C and a time of 1.5h. Figure 1 As shown, the alloy consists of face-centered cubic Be 95.65 W 4.35 And four parties Be 92.31 W 7.69 Phase composition, grain size ≤80um, neutron multiplication rate between 0.92 and 0.96, excellent high temperature performance and radiation swelling resistance, the properties are shown in Table 1, indicating that the alloy is particularly suitable for neutron multiplication and high temperature fields.
[0063] Table 1:
[0064]
[0065] The properties in Table 1 are described as follows.
[0066] Neutron multiplication performance refers to the neutron multiplication performance of the elements that constitute the alloy, and is evaluated by the neutron multiplication rate. Considering that beryllium is a naturally excellent neutron multiplication material, beryllium is used as a comparison material (the neutron multiplication rate is set to 1). The closer the performance of other materials is to 1, the better the neutron multiplication performance.
[0067] Tritium retention performance (after tritium is injected into the material, its retention in the material can be measured, which is an important material performance). Since the purpose of fusion neutron breeder is to achieve self-sustaining tritium fuel, the retention of tritium in the material is also very important. The temperature desorption gas analyzer (TDS) is used to measure the tritium retention. That is, according to the degree of tritium retention, it can be excellent (very little retention), medium (partial retention), and poor (a lot of retention).
[0068] Anti-radiation swelling performance. Neutron irradiation materials will produce a large number of vacancies. These vacancies will further migrate and aggregate to form vacancy clusters such as holes, causing the volume swelling of the material. Under the conditions of high temperature 400℃ and helium injection of 3000appm, the irradiation swelling rate of metallic beryllium is >3%, endangering the safe operation of the reactor. It is assumed to have poor anti-swelling performance, and it is used as a comparison. The irradiation swelling rate is 1-3%, which is medium, and the irradiation swelling rate is less than 1%, which is excellent.
[0069] Other properties are well known in the industry and will not be specifically described. Due to differences in material composition, heat treatment process, hot and cold processing process, etc., the phase composition and grain size of the material are different, thereby regulating various properties of the material. For example, the alloy No. 1 in Table 1, which is composed of beryllium and titanium, can be obtained by proper annealing to obtain single-phase Be 92.31 Ti7.69 The single phase is a tetragonal structure phase. Its neutron multiplication rate is measured to be 0.92, and its tritium retention performance is excellent. However, its fracture toughness and processing performance are particularly poor, and its later ball formation rate is particularly low, which seriously limits its application. The present invention uses beryllium and tungsten as the main elements, supplemented by other elements such as Re and Zr, and utilizes neutron multiplication nuclides such as Be, Zr, large-sized atomic refractory metal elements, low-activation elements such as W, Re, etc., and auxiliary phases such as Be 95.65 Re 4.35 The grain size of the material is controlled by combining processes such as the neutron multiplication rate of beryllium tungsten alloy.
[0070] Example 2
[0071] A high temperature and high neutron multiplication rate beryllium tungsten alloy, the composition of which is: Be: 93.74at.%, W: 4.26at.%, O: 0.97at.%, other elements including C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, etc., with a total content of 1.03at.%, is prepared by hot isostatic pressing, temperature 1000℃, time 1.5h, 1200℃ vacuum annealing for 2h, the alloy is face-centered cubic Be 95.65 W 4.35 The composition increases the proportion of neutron multiplying nuclide beryllium, the grain size is <80um, the neutron multiplication rate is as high as 0.96, the high temperature performance and radiation swelling resistance are excellent, and the properties are shown in Table 1, indicating that the alloy is particularly suitable for the field of neutron multiplication.
[0072] Example 3
[0073] A high temperature and high neutron multiplication rate beryllium tungsten alloy, the composition of which is: Be: 90.46at.%, W: 7.54at.%, O: 0.97at.%, other elements including C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, etc., with a total content of 1.03at.%, is prepared by hot isostatic pressing, temperature 1000℃, time 1.5h, 1200℃ vacuum annealing 3.5h, the alloy is composed of tetragonal Be 92.31 W 7.69 The composition, grain size <80um, neutron multiplication rate is 0.92, high temperature performance and anti-irradiation swelling performance are excellent, and the properties are shown in Table 1, indicating that the alloy is suitable for the neutron multiplication field and high temperature field.
[0074] Example 4
[0075] A high temperature and high neutron multiplication rate beryllium tungsten alloy, the composition of which is: Be: 89.52at.%, W: 8.28at.%, O: 1.01at.%, other elements including C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, etc., the total content is 1.19at.%, and the alloy is prepared by plasma sintering at a temperature of 1000°C and a time of 1.0h. 92.31 W 7.69 and W phases, with a grain size of <80um, a neutron multiplication rate between 0.67 and 0.92, excellent high temperature performance and anti-irradiation swelling performance. The properties are shown in Table 1, indicating that the alloy is suitable for the neutron multiplication field and high temperature field.
[0076] Example 5
[0077] A high temperature and high neutron multiplication rate beryllium tungsten alloy, the composition of which is: Be: 65.33at.%, W: 32.67at.%, O: 0.97at.%, other elements including C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, etc., with a total content of 1.03at.%, is prepared by hot isostatic pressing, temperature 1200℃, time 1.5h, 1400℃ vacuum annealing 3.0h, the alloy is composed of hexagonal Be 66.67 W 33.33 Phase composition, grain size <80um, neutron multiplication rate of 0.67, high temperature performance and anti-irradiation swelling performance are excellent, the properties are shown in Table 1, indicating that the alloy is particularly suitable for high temperature fields.
[0078] Example 6
[0079] A high temperature and high neutron multiplication rate beryllium tungsten alloy, the composition of which is: Be: 93.74at.%, W: 2.21at.%, Re: 2.05at.%, O: 0.97at.%, other elements include Si, S, Al, Fe, Mg, As, Ti, Cr, Mn, Co, Ni, Cu, W, U, etc. The total content is 1.03at.%, and the alloy is prepared by hot isostatic pressing at a temperature of 1000°C for 1.5 hours and vacuum annealing at 1200°C for 2 hours. 95.65 W 4.35 and Be 95.65 Re 4.35 Phase composition, grain size <80um, neutron multiplication rate up to 0.96, excellent high temperature performance and anti-irradiation swelling performance, the properties are shown in Table 1, indicating that the alloy is particularly suitable for neutron multiplication and high temperature fields.
[0080] The above description shows and describes several preferred embodiments of the present invention, but as mentioned above, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not depart from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
Claims
1. A beryllium-tungsten alloy with high temperature, high toughness and high neutron multiplication rate, characterized in that: The atomic percentage expression of the beryllium-tungsten alloy material composition is Be a (W b M c )X d , where M is Re, X is one or more of O, C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, 63 ≤ a ≤ 97, 3 ≤ b ≤ 37, 0 < c ≤ 37, 0 ≤ d ≤ 3, and a + b + c + d = 100.
2. The high-temperature, high-toughness, high-neutron multiplication rate beryllium-tungsten alloy according to claim 1, characterized in that: When 0 < d ≤ 2, 0 < c ≤ 2.17, c < b ≤ 4.35, 93.65 ≤ a ≤ 97, the beryllium tungsten alloy includes a face-centered cubic structure phase and a hexagonal close-packed structure phase, and the grain size ≤ 80 μm.
3. The high-temperature, high-toughness, high-neutron multiplication rate beryllium-tungsten alloy according to claim 1, characterized in that: When d = 0, 0 < c ≤ 2.17, 0 < c < b ≤ 4.35, and a = 95.65, the atomic percentage expression of the beryllium tungsten alloy material composition is Be 95.65 (W,M) 4.35 , and the beryllium tungsten alloy is a face-centered cubic structure with a grain size ≤ 80 μm.
4. The high-temperature, high-toughness, high-neutron multiplication rate beryllium-tungsten alloy according to claim 1, characterized in that: When 0 < d ≤ 2, 0 < c ≤ 18.5, c < b ≤ 37, 61 ≤ a < 92.31, the beryllium tungsten alloy includes a tetragonal structure phase and a hexagonal structure phase, and the grain size ≤ 80 μm.
5. The high temperature, high toughness and high neutron proliferation rate beryllium tungsten alloy according to claim 1, characterized in that: When d=1.98, c=1.75, b=7.41, a=88.86, the atomic percentage expression of the composition of the beryllium tungsten alloy material is Be 88.86 W 7.41 M 1.75 X 1.98 , including tetragonal structure phase and hexagonal structure phase, with grain size ≤80um.
6. The high-temperature, high-toughness, high-neutron multiplication rate beryllium-tungsten alloy according to claim 1, characterized in that: When 0 < d ≤ 2, 0 < c ≤ 3.84, c < b ≤ 7.69, 90.31 < a < 95.65, the beryllium tungsten alloy is a face-centered cubic and tetragonal structure phase, and the grain size ≤ 80 μm.
7. The high temperature, high toughness and high neutron multiplication rate beryllium tungsten alloy according to claim 1, characterized in that: When d=1.98, c=1.75, b=2.51, a=93.76, the atomic percentage expression of the composition of the beryllium tungsten alloy material is Be 93.76 W 2.51 M 1.75 X 1.98 , it has a face-centered cubic structure and the grain size is ≤80um.
8. Application of the beryllium tungsten alloy with high temperature, high toughness and high neutron multiplication rate according to any one of claims 1-7 in a neutron multiplier for a fusion reactor.
Citation Information
Patent Citations
Material including beryllium intermetallic compound and having excellent high-temperature property applied to nuclear fusion reactor
US20050135960A1