Hydrogenation catalyst suitable for high temperature section and preparation method and application thereof, hydrodesulfurization method
By loading specific metal elements and phosphorus elements on the alumina carrier and controlling the pore size distribution, a hydrogenation catalyst suitable for the high-temperature section is prepared, which solves the problem of existing catalysts being easily deactivated at high temperatures and achieves efficient hydrodesulfurization. The response and stability are improved to meet the stringent response requirements of the National VI standards.
Patent Information
- Application Number
- CN202111265082.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Existing hydrogenation catalysts are prone to deactivation in high-temperature environments, resulting in shortened operating cycles of diesel hydrogenation units and poor stability, making it difficult to meet the stringent reaction requirements of the National VI standards.
Develop a hydrogenation catalyst suitable for the high-temperature section. By loading Group VIII metal elements, Group VIB metal elements and phosphorus elements on an alumina carrier, the pore size of the catalyst is controlled to present a unimodal pore distribution in the range of 8-20nm. , using an impregnation method to introduce metal precursors and phosphorus compounds, and adding organic alcohol compounds and carboxylic acid compounds during the drying process to prepare a catalyst with good activity and stability.
It extends the operating cycle of the catalyst, improves the activity and stability of the hydrodesulfurization reaction, reduces the carbon deposition rate of the catalyst, is suitable for hydrodesulfurization reactions under high temperature conditions, and significantly improves the operating efficiency and performance of the diesel hydrogenation unit. life.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrogenation catalyst preparation, and in particular to a hydrogenation catalyst suitable for a high temperature section, a preparation method and application thereof, and a hydrogenation desulfurization method. Background Art
[0002] In the past five years, with the increasing awareness of environmental protection in society, my country's diesel quality standards have been rapidly upgraded to the National VI standard, requiring the sulfur content and polycyclic aromatic hydrocarbons in diesel to be reduced to 10 mg / kg and 7% respectively. Based on the existing technology, the production of diesel that meets the National VI standard requires an increase in the severity of the reaction, which will greatly increase the deactivation rate of the catalyst and seriously shorten the operation cycle of the unit. The development of high-performance catalysts and grading technology is a more economical solution. The industrial diesel hydrogenation unit is an adiabatic reactor. During the diesel hydrogenation reaction, the occurrence of hydrodesulfurization and aromatic saturation reactions is an exothermic reaction, and the industrial reaction temperature rise is generally 30-60°C. In addition, as the catalyst gradually deactivates, the reaction temperature gradually rises. The reaction environment of some catalysts in the industrial diesel hydrogenation unit is a continuous high temperature environment. However, high temperature reactions will accelerate the deactivation of the catalyst. Therefore, the development of high-performance catalysts that adapt to the high temperature section of the hydrogenation reaction plays an important role in promoting the operation cycle of the unit.
[0003] Patent application with application number 202010395989.6 discloses a hydrorefining catalyst and its preparation method and application. The catalyst includes 50-80wt% of a carrier and 20-50wt% of an active metal component. The carrier uses a composite oxide to regulate the interaction force between the active metal and the carrier in the catalyst, thereby increasing the concentration of active hydrogen species on the active metal surface and improving the hydrodesulfurization and hydrodenitrogenation reaction activity of the catalyst.
[0004] Patent application No. 201811455219.5 discloses a method for preparing a supported hydrogenation catalyst, wherein one or more of the group consisting of ethylenediaminetetramethylene phosphate, tetrabutylammonium fluoride and tartaric acid are used as active metal positioning loading directing agents, and a γ-Al2O3 carrier is contacted with a solution containing the active metal positioning loading directing agent to prepare a catalyst, wherein the catalyst has high hydrodesulfurization, denitrogenation activity and aromatic saturation activity.
[0005] The patent application with application number 201711023399.5 discloses a diesel hydrorefining catalyst, comprising 1-30% TS-1 molecular sieve, 20-50% γ-Al2O3, 0.01-10% zirconium oxide, 0.01-5% graphene, 10-40% heteropoly acid calculated as metal oxide, and the catalyst specific surface area is 250-500m 2 / g, pore volume 0.5-0.8mL / g. The catalyst has high hydrodesulfurization activity.
[0006] Patent application No. 201710984468.2 discloses a bulk hydrorefining catalyst, comprising metal components of W, Ni and Mo. The preparation steps of the catalyst include 1) conducting a gelling reaction of a mixed solution A containing Ni, W and Al, an organic additive and a precipitant in parallel, and aging the resulting slurry; 2) then adding a mixed solution B containing W and Al, a MoO3 slurry and a precipitant in parallel to the aged slurry, and then aging; 3) drying, molding and other steps; the catalyst has high hydrodesulfurization and hydrodenitrogenation reaction activity, especially for treating diesel feedstocks with high nitrogen and high sulfur content.
[0007] From the above, it can be seen that the research and invention of diesel hydrodesulfurization catalysts have improved the properties of catalysts from many angles, and significantly improved the activity of diesel hydrodesulfurization catalysts. However, the prior art rarely discloses hydrogenation catalysts or technologies for the high temperature section of diesel hydrotreating units. Summary of the invention
[0008] The purpose of the present invention is to overcome the problems of the prior art that the hydrogenation catalyst is easily deactivated and has poor stability under high-temperature use environment, and to provide a hydrogenation catalyst suitable for the high-temperature section and its preparation method and application, and a hydrodesulfurization method. The catalyst is particularly suitable for hydrodesulfurization treatment in the high-temperature section, and the catalyst has good activity and stability.
[0009] In order to achieve the above-mentioned object, the first aspect of the present invention provides a hydrogenation catalyst suitable for a high temperature section, wherein the catalyst comprises alumina and a metal element of Group VIII and a metal element of Group VIB supported on the alumina and a phosphorus element, wherein the pore size of the catalyst is in the range of 8-20 nm and presents a unimodal pore distribution; the catalyst composition is as follows: (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.18-0.39nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA supis the specific surface area of the carrier.
[0010] Preferably, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.25-0.38nm.
[0011] The second aspect of the present invention provides a method for preparing the hydrogenation catalyst suitable for the high temperature section described in the first aspect, the method comprising: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound and optionally an organic alcohol compound and / or a carboxylic acid compound containing -OH into alumina by an impregnation method, and then drying.
[0012] The third aspect of the present invention provides use of the hydrogenation catalyst suitable for the high temperature section described in the first aspect in a hydrodesulfurization reaction.
[0013] The fourth aspect of the present invention provides a hydrodesulfurization method, which comprises: under hydrodesulfurization conditions, contacting the distillate oil with a catalyst for reaction, wherein the catalyst is the hydrogenation catalyst suitable for the high temperature section as described in the first aspect.
[0014] The inventors found in their research that during the diesel hydrogenation reaction, as the operating time increases, the catalyst will gradually deactivate. As the reaction temperature increases, the catalyst deactivation rate will gradually accelerate. The industrial diesel hydrogenation unit is an adiabatic reactor, and the lower bed layer of the reaction is always in a high-temperature reaction environment, and the catalyst is very easy to deactivate. Therefore, reducing the deactivation rate of the catalyst in the high-temperature section of the diesel hydrogenation unit will greatly extend the catalyst's operating cycle and bring more profits to the diesel hydrogenation unit.
[0015] In the present invention, the carrier used in the hydrogenation catalyst has a pore structure of different sizes, and the reactant molecules need to smoothly pass through the contact active center during the reaction. At a higher reaction temperature, the speed of the reactant molecules in the active center reaction increases, and only when the pores of the catalyst are relatively unobstructed can the products generated by the reaction diffuse out of the reaction center faster. If the reactant molecules cannot quickly leave the active center, the reactants cannot diffuse in faster, so the tendency of catalyst coking will increase, affecting the stability of the catalyst. Therefore, the catalyst should have a higher number of active centers on the one hand, and on the other hand should have a more spacious pore to promote the diffusion of reactants and products and thus reduce the deactivation rate of the catalyst.
[0016] In the present invention, by controlling the composition of the hydrogenation catalyst, and then controlling the pore structure and active metal loading of the catalyst, a hydrogenation catalyst suitable for a high temperature section is provided, and the hydrogenation catalyst has good activity and stability. DETAILED DESCRIPTION
[0017] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0018] The first aspect of the present invention provides a hydrogenation catalyst suitable for a high temperature section, wherein the catalyst comprises an alumina carrier and a metal element of Group VIII and a metal element of Group VIB supported on the alumina and a phosphorus element, wherein the pore size of the catalyst is in the range of 8-20 nm and presents a unimodal pore distribution; the catalyst composition is as follows: (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.18-0.39nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of the carrier.
[0019] In a preferred case, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.25-0.38nm.
[0020] In the present invention, ρMoO3, ρWO3, ρNiO, ρCoO, and ρP2O5 are 4.69 g / cm 3 , 7.16g / cm 3 、6.67g / cm 3 、6.45g / cm 3 and 2.39 g / cm 3 calculate.
[0021] In the present invention, the composition of the catalyst is specifically limited so that the amount of each raw material is added according to the above expression, and finally a hydrogenation catalyst suitable for the high temperature section with satisfactory performance is obtained.
[0022] The above expression is used to limit the composition of the catalyst. On the one hand, it can meet the requirements of catalyst activity. On the other hand, it can ensure that the pores of the catalyst remain at a large level after the active metal components of the catalyst are loaded on the alumina carrier, forming an unobstructed diffusion channel, slowing down the carbon deposition of the catalyst, and promoting the stability of the hydrogenation catalyst at high temperature.
[0023] In the present invention, the catalyst has specific physical parameters and is particularly suitable for high temperature hydrogenation reactions. Preferably, the specific surface area of the catalyst is 185-210 m 2 / g.
[0024] In a preferred case, in the catalyst, the volume of pores with a pore size distribution of 8-20 nm accounts for 50-80% of the total pore volume of the catalyst, preferably 60-75%. The advantage of adopting this preferred embodiment is that it provides a larger diffusion channel for the reaction, which can slow down the carbon deposition rate of the catalyst on the one hand, and improve the volumetric carbon deposition capacity of the catalyst on the other hand, thereby promoting the stability of the catalyst under high temperature reaction conditions.
[0025] In a preferred embodiment, the average pore size of the catalyst is 6-18 nm, more preferably 8-12 nm.
[0026] In a preferred embodiment, the pore volume of the catalyst is 0.4-0.6 cm 3 / g, more preferably 0.4-0.5cm 3 / g.
[0027] In the present invention, the 2-6nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 6nm, the 2-4nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 4nm, the 4-6nm pores refer to pores with a pore diameter greater than or equal to 4nm and less than 6nm, and the 8-20nm pores refer to pores with a pore diameter greater than or equal to 8nm and less than 20nm.
[0028] In the present invention, the specific surface area, pore distribution, pore volume and average pore diameter of the catalyst are measured after calcination at 400° C. for 3 hours.
[0029] In the present invention, the specific surface area, pore distribution, pore diameter and pore volume of the catalyst are measured by low temperature nitrogen adsorption method (BET).
[0030] In the present invention, in order to make the hydrogenation catalyst suitable for high temperature hydrodesulfurization reaction, an alumina carrier with specific physicochemical parameters is selected. Preferably, the water absorption rate of the alumina is greater than 0.9 mL / g, more preferably 0.9-1.1 mL / g, and the specific surface area is greater than 260 m 2 / g, more preferably 270-280m 2 / g, the average pore size is greater than 8nm, more preferably 10-12nm, and the pore distribution morphology is a unimodal pore distribution.
[0031] In a preferred embodiment, in the alumina, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina, preferably no more than 8%, and more preferably no more than 5%.
[0032] In a preferred embodiment, in the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 4%, preferably no more than 1% of the total pore volume of the alumina.
[0033] The advantages of using alumina within the above preferred range as a carrier mainly include: 1) providing a larger specific surface area to promote the dispersion of the active phase; 2) providing a larger reaction channel to promote better contact of the reaction molecules with the active center at high temperature; 3) minimizing the smaller pore size, promoting uniform pore size, reducing the formation of carbon deposits, promoting volumetric carbon capacity, and improving the stability of the catalyst.
[0034] In the present invention, the Group VIII metal element includes but is not limited to at least one of Fe, Co and Ni, preferably Co and / or Ni.
[0035] In a preferred embodiment, the VIB Group metal element includes but is not limited to at least one of Cr, Mo and W, preferably Mo and / or W.
[0036] In the present invention, there is no specific restriction on the amount of the VIB group metal element and the phosphorus element in the catalyst, as long as the performance of the hydrogenation catalyst can be met. Preferably, the molar ratio of Zi / Xi in the catalyst is 0.1-0.35:1, preferably 0.2-0.35:1. The advantage of adopting this preferred embodiment is that it can promote the dissolution of the active component, maintain a moderate amount of phosphate, and promote the dispersion of the active metal.
[0037] In a preferred embodiment, the atomic concentration of the metal element of Group VIB in the catalyst on the surface of the carrier is 2-6 atom / nm 2 , preferably 3-4.5atom / nm 2 .
[0038] In the present invention, atomic concentration refers to the average atomic concentration of the metal element of Group VIB on the surface of the carrier, which is obtained by measuring the metal loading and the specific surface area of the carrier and then calculating. For example, it can be obtained by the following calculation formula: atomic concentration = (a / M Xi )×N A / (1×SA sup ), where N A is Avogadro's constant, ai is the mass relative to 1 gram of carrier Xi, M Xi is the molecular weight of Xi, SA sup The advantage of using the atomic concentration within this range is that a moderate number of active centers are formed, which on the one hand meets the needs of the reaction, and on the other hand leaves enough space to achieve the purpose of promoting diffusion and reducing carbon deposition.
[0039] In the present invention, there is no specific restriction on the amount of the metal element of Group VIB in the catalyst. Preferably, the atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the catalyst is 0.2-0.4, preferably 0.2-0.35. This preferred embodiment can better promote the synergistic effect of the metal element of Group VIB and the metal element of Group VIII, and meet the requirements of hydrogenation activity at high temperature.
[0040] In the present invention, the catalyst further comprises an alcohol compound and / or a carboxylic acid compound. Preferably, the catalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds containing -OH, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds containing -OH to the metal element of Group VIII is 1-6, preferably 2-5. The purpose of adopting this preferred embodiment is to ensure the high dispersibility of the metal element of Group VIII, weaken the interaction between the carrier and the metal, promote the generation of more active phases, and improve the activity of the catalyst.
[0041] In a preferred case, the organic alcohol compound containing -OH can be at least one of a monohydric alcohol, a dihydric alcohol and a polyhydric alcohol. In a particularly preferred case, the organic alcohol compound containing -OH is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane. In a more particularly preferred case, the organic alcohol compound containing -OH is selected from one of glycerol and propanol.
[0042] In a preferred embodiment, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, and is further preferably at least one of formic acid, citric acid and acetic acid.
[0043] In a particularly preferred embodiment, the catalyst comprises one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol, trimethylolethane and / or formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid, tartaric acid.
[0044] In the present invention, there is no specific limitation on the size of the catalyst. Preferably, the equivalent diameter of the catalyst is 0.5-1.8 mm, more preferably 0.8-1.6 mm.
[0045] In the present invention, there is no specific limitation on the shape of the catalyst, and conventional catalyst shapes in the art are applicable to the present invention. Preferably, the catalyst is cylindrical, clover, four-leaf clover, butterfly, honeycomb or other irregular shapes, more preferably butterfly.
[0046] The second aspect of the present invention provides a method for preparing the high temperature section hydrogenation catalyst according to the first aspect, the method comprising:
[0047] The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the alumina by an impregnation method, and then dried.
[0048] In the present invention, an organic alcohol compound and / or a carboxylic acid compound containing -OH may or may not be introduced. In the present invention, an organic alcohol compound and / or a carboxylic acid compound containing -OH is preferably introduced.
[0049] In the present invention, the types of Group VIII metals, Group VIB metals, -OH-containing organic alcohol compounds, and carboxylic acid compounds have been described in the first aspect and will not be elaborated on here.
[0050] In the present invention, preferably, the VIB Group metal precursor includes but is not limited to one or more of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate and tungsten oxide.
[0051] In a preferred embodiment, the Group VIII metal precursor includes, but is not limited to, one or more of cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.
[0052] In a preferred embodiment, the phosphorus-containing compound includes, but is not limited to, one or more of phosphoric acid, hypophosphorous acid, ammonium phosphate and diammonium phosphate.
[0053] In a preferred embodiment, the amount of the Group VIII metal precursor, the Group VIB metal precursor, and the phosphorus-containing compound is such that the catalyst obtained satisfies the above (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value required.
[0054] According to the preparation method of the present invention, there is no specific limitation on the impregnation method, and conventional impregnation methods in the art are applicable to the present invention. For example, it can be one of co-impregnation, step-by-step impregnation, saturated impregnation and supersaturated impregnation. In a preferred embodiment, the catalyst is prepared by co-impregnation in the present invention. In a more preferred embodiment, the impregnation method comprises: impregnating the alumina with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound containing -OH and / or a carboxylic acid compound.
[0055] In the present invention, there is no specific limitation on the order of adding the Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound, and the optionally -OH-containing organic alcohol compound and / or the carboxylic acid compound, as long as it is conducive to uniform mixing of the components. In a preferred embodiment, the Group VIII metal precursor, the Group VIB metal precursor, and the -OH-containing organic alcohol compound and / or the carboxylic acid compound are added to an aqueous solution of the phosphorus-containing compound to prepare the impregnation solution. In the present invention, the order of adding the -OH-containing organic alcohol compound and / or the carboxylic acid compound, the phosphorus-containing compound, and the metal precursor can also be interchanged.
[0056] The present invention does not particularly limit the preparation method of the hydrogenation catalyst, and those skilled in the art can select it according to conventional means. In order to facilitate the understanding of the technical solution of the present invention, an exemplary description is now provided to reflect the preparation method of the present invention, and the method of the present invention includes but is not limited to this. For example, the hydrogenation catalyst can be prepared by the following preparation method: (1) According to the atomic concentration of the VIB group metal element and the specific surface area of alumina, the feeding amount of the VIB group metal precursor per gram of alumina is determined; (2) According to the atomic ratio of the VIII group metal element to the total amount of the VIII group metal element and the VIB group metal element, the feeding amount of the VIII group metal precursor per gram of alumina is determined; (3) According to (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The content of the phosphorus-containing compound is calculated based on the value of , and then the amount of the phosphorus-containing compound per gram of the carrier is determined; (4) the amount of the organic alcohol compound and / or the carboxylic acid compound containing -OH is calculated based on the molar ratio of the organic alcohol compound and / or the carboxylic acid compound containing -OH to the metal element of Group VIII; (5) according to the amount of the above-mentioned Group VIB metal precursor, Group VIII metal precursor, phosphorus-containing compound and organic alcohol compound and / or carboxylic acid compound containing -OH, the alumina is impregnated with the impregnation solution according to the pore saturation impregnation method, and then dried. Specifically, a phosphorus-containing compound is first dissolved in water to obtain a phosphorus-containing aqueous solution, and then an organic alcohol compound and / or a carboxylic acid compound containing -OH, a VIB group metal precursor and a VIII group metal precursor are added, and the mixture is stirred under heating until it is completely dissolved, and the temperature is maintained to obtain an impregnation solution; (6) the water absorption rate of alumina is measured, and the liquid absorption rate of alumina is calculated according to the formula of water absorption rate of alumina-0.1; (7) according to the liquid absorption rate of alumina, the volume of the impregnation solution is adjusted to a corresponding volume (alumina liquid absorption rate×carrier mass), and the impregnation solution and a corresponding mass of alumina are evenly mixed and allowed to stand, and then dried to prepare a hydrogenation catalyst.
[0057] In the present invention, the specific conditions for drying have a wide range of selection, and those skilled in the art can select according to actual needs. Preferably, the drying conditions include: a temperature of 80-200° C. and a time of 1-10 h.
[0058] The third aspect of the present invention provides use of the hydrogenation catalyst suitable for the high temperature section described in the first aspect in a hydrodesulfurization reaction.
[0059] The fourth aspect of the present invention provides a hydrodesulfurization method, which comprises contacting a distillate oil with a catalyst under hydrodesulfurization conditions, wherein the catalyst is the hydrogenation catalyst suitable for the high temperature section as described in the first aspect.
[0060] In a preferred embodiment, the hydrodesulfurization conditions include: pressure of 3-14 MPa, temperature of 350-410°C, volume space velocity of 0.5-10 hours -1 , the volume ratio of hydrogen to oil is 200-1000:1; the preferred temperature is 360-400℃.
[0061] In a particularly preferred case, the temperature of the hydrodesulfurization reaction of the hydrogenation catalyst is 370-390° C. The hydrogenation catalyst of the present invention is particularly suitable for the hydrodesulfurization reaction in the high temperature section. In the hydrodesulfurization reaction, the hydrogenation catalyst can maintain good activity and stability.
[0062] According to the hydrodesulfurization method provided by the present invention, preferably, before the contacting, the distillate oil is first subjected to a first contact reaction with a first hydrogenation catalyst, and then subjected to a contact reaction with the hydrogenation catalyst suitable for the high temperature section provided by the present invention.
[0063] Preferably, the packing volume ratio of the first hydrogenation catalyst and the hydrogenation catalyst suitable for the high temperature section provided by the present invention is 1:0.25-1.5.
[0064] The first hydrogenation catalyst may be any hydrodesulfurization catalyst conventionally used in the art, and may be commercially available or prepared by the user, and the present invention will not elaborate on this.
[0065] Preferably, the conditions of the first contact reaction include: pressure of 3-14 MPa, temperature of 300-380°C, volume space velocity of 1-6 hours -1 , the volume ratio of hydrogen to oil is 200-1200:1.
[0066] In the present invention, the hydrodesulfurization reaction of the hydrogenation catalyst is measured on a high-pressure small-scale reactor, the upper bed is filled with industrial catalyst, and the lower bed is filled with the hydrogenation catalyst suitable for the high temperature section described in the first aspect of the present invention.
[0067] In a preferred embodiment, the sulfur content in the distillate oil is 5000-30000 ppm.
[0068] In a preferred case, the catalyst needs to be converted from an oxidized catalyst to a sulfurized catalyst by sulfurization before use. In the present invention, there is no specific limitation on the sulfurization method, and conventional sulfurization methods in the art are applicable to the present invention. Preferably, for example, it can be one of dry sulfurization and wet sulfurization. There is no particular limitation on the type of the vulcanizing agent, and those skilled in the art can select it according to conventional schemes in the art.
[0069] In a preferred embodiment, the vulcanization conditions include: vulcanization temperature of 280-420°C, heating rate of 5-60°C / hour, time of 10-48h, pressure of 0.1-15MPa, volume space velocity of 0.5-20h -1 , the volume ratio of hydrogen to oil is 100-2000:1.
[0070] The present invention will be described in detail below through examples. In the following examples, the hydrodesulfurization performance of the catalyst is measured on a high-pressure small-scale reactor, the upper bed is filled with 6 mL of an industrial catalyst, which is composed of 4.3% by weight of NiO, 27% by weight of MoO3, and 68.7% by weight of alumina, and the lower bed is filled with 10 mL of the hydrogenation catalyst suitable for the high temperature section of the present invention, and the oxidized catalyst is directly converted into a sulfurized catalyst by a programmed temperature sulfurization method. The sulfurization conditions are: the sulfurization pressure is 6.4 MPa, the sulfurized oil is kerosene containing 2% by weight of CS2, and the volume space velocity is 2 hours -1 , the hydrogen-to-oil volume ratio is 300v / v, first keep the temperature at 230℃ / h for 6h, then heat it up to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials for hydrodesulfurization activity test, the reaction raw materials are distillate oil with a sulfur content of 10890ppm. The test conditions are: pressure of 6.4MPa, volume space velocity of 1.875h -1 , the volume ratio of hydrogen to oil was 300 v / v, and the reaction temperature was 370°C. The properties of the product were analyzed after the reaction was stable for 2 days. In order to examine the stability of the catalyst, the mass fraction of sulfur in the reaction product was kept at 10 ppm, the reaction temperature was adjusted every day, and the operation was continued for 5 days. The changes in the reaction temperature before and after 5 days were compared to measure the stability of the catalyst.
[0071] The composition of the catalyst is calculated based on the feed amount. The pore distribution, pore size and pore volume of 2-100 nm in the catalyst and the carrier are determined by low temperature nitrogen adsorption method (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The sulfur mass fraction in the product is analyzed using a sulfur nitrogen analyzer (produced by Thermo Fisher, model TN / TS3000).
[0072] Example 1
[0073] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of 280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.
[0074] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0075] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0076] The atomic concentration of Mo in the catalyst is 4.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.346nm, and the molar ratio of glycerol to Ni is 2.
[0077] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 192m 2 / g, pore volume 0.45cm 3 / g, the average pore size is 9.4nm, the pore volume with a pore size distribution of 8-20nm accounts for 63.0% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single peak pore distribution in the range of 8-20nm. After the catalyst was sulfurized and tested for reaction, the sulfur content in the product was 5.7ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.3℃ after 5 days of reaction.
[0078] Example 2
[0079] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of 280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.
[0080] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0081] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0082] The atomic concentration of Mo in the catalyst is 3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.3, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.26 nm, and the molar ratio of glycerol to Ni is 5.
[0083] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption. The specific surface area of the catalyst is 210m 2 / g, pore volume 0.5cm 3 / g, the average pore size is 9.5nm, the pore volume with a pore size distribution of 8-20nm accounts for 65.8% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single peak pore distribution in the range of 8-20nm. After the catalyst is sulfurized and reacted, the sulfur content in the product is 9.8ppm. When the sulfur content of the product is kept at 10ppm, the reaction temperature rises by 1.5℃ after 5 days of reaction.
[0084] Example 3
[0085] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of 280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.
[0086] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 4 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0087] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0088] The atomic concentration of Mo in the catalyst is 3.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi) / SA sup The nanostructured carbon fiber is 0.29 nm, and the molar ratio of glycerol to Ni is 3.
[0089] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 204m 2 / g, pore volume 0.48cm 3 / g, the average pore size is 9.4nm, the pore volume with a pore size distribution of 8-20nm accounts for 66.2% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single-peak pore distribution in the range of 8-20nm. After the catalyst was sulfurized and reacted, the sulfur content in the product was 8.7ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.4℃ after 5 days of reaction.
[0090] Example 4
[0091] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of 280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.
[0092] A certain amount of ammonium metatungstate, basic nickel carbonate and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0093] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0094] The atomic concentration of W in the catalyst is 4atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.35, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.38 nm, and the molar ratio of citric acid to Ni is 2.
[0095] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 170m 2 / g, pore volume 0.4cm 3 / g, the average pore size is 9.4nm, the pore volume with a pore size distribution of 8-20nm accounts for 65.8% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single peak pore distribution in the range of 8-20nm. After the catalyst was sulfurized and tested for reaction, the sulfur content in the product was 4.6ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.6℃ after 5 days of reaction.
[0096] Example 5
[0097] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of 270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-2nm accounts for 73.5% of the total pore volume.
[0098] A certain amount of MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 4 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0099] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0100] The atomic concentration of Mo in the catalyst is 4.2atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.32, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.37 nm, and the molar ratio of citric acid to Ni is 2.
[0101] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 189m 2 / g, pore volume 0.48cm 3 / g, the average pore size is 10.2nm, the pore volume with a pore size distribution of 8-20nm accounts for 69.5% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single peak pore distribution in the range of 8-20nm. After the catalyst is sulfurized and tested for reaction, the sulfur content in the product is 7.8ppm. When the sulfur content of the product is kept at 10ppm, the reaction temperature increases by 1.8℃ after 5 days of reaction.
[0102] Example 6
[0103] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of 270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm, accounting for 73.5%.
[0104] A certain amount of MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0105] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0106] The atomic concentration of Mo in the catalyst is 4.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.36 nm, and the molar ratio of citric acid to Ni is 2.
[0107] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 190m 2 / g, pore volume 0.47cm 3 / g, the average pore size is 9.9nm, the pore volume with a pore size distribution of 8-20nm accounts for 72.6% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single peak pore distribution in the range of 8-20nm. After the catalyst was sulfurized and tested for reaction, the sulfur content in the product was 6.5ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.9℃ after 5 days of reaction.
[0108] Comparative Example 1
[0109] The same carrier as in Example 1 was selected to prepare a catalyst. A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0110] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0111] The atomic concentration of Mo in the catalyst is 2atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.22, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.17 nm, and the molar ratio of glycerol to Ni is 2.
[0112] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 230m 2 / g, pore volume 0.58cm 3 / g, the average pore size is 10.1nm, the pore volume with a pore size distribution of 8-20nm accounts for 66.2% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single-peak pore distribution in the range of 8-20nm. After the catalyst was sulfurized and reacted, the sulfur content in the product was 29.5ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.8℃ after 5 days of reaction.
[0113] Comparative Example 2
[0114] The same carrier as in Example 1 was selected to prepare a catalyst. A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0115] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0116] The atomic concentration of Mo in the catalyst is 1.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.15, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.11 nm, and the molar ratio of glycerol to Ni is 2.
[0117] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 248m 2 / g, pore volume 0.62cm 3 / g, the average pore size is 9.9nm, the pore volume with a pore size distribution of 8-20nm accounts for 64.2% of the total pore volume of the catalyst, and the pore size of the catalyst presents a single-peak pore distribution in the range of 8-20nm. After the catalyst was sulfurized and tested for reaction, the sulfur content in the product was 39.2ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.7℃ after 5 days of reaction.
[0118] It can be seen from the data of the embodiments and comparative examples that the hydrogenation catalyst suitable for the high temperature section provided by the present invention has high stability and activity under high temperature reaction conditions when placed in the lower bed layer, is particularly suitable for hydrodesulfurization reactions under high temperature conditions, and has good industrial application prospects.
[0119] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A hydrogenation catalyst suitable for a high temperature section, wherein: The catalyst comprises alumina, and a metal element of Group VIII and a metal element of Group VIB, and a phosphorus element supported on the alumina, wherein the pore size of the catalyst presents a unimodal pore distribution in the range of 8-20 nm; Catalyst composition according to (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, where Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.18-0.39nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of the carrier; The specific surface area of the catalyst is 185-210m 2 / g; In the catalyst, the pore volume with a pore size distribution of 8-20 nm accounts for 50-80% of the total pore volume of the catalyst; The average pore size of the catalyst is 6-18 nm; The pore volume of the catalyst is 0.4-0.6 cm 3 / g.
2. The catalyst according to claim 1, wherein (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.25-0.38nm.
3. The catalyst according to claim 1, wherein In the catalyst, the pore volume with pore size distribution between 8 and 20 nm accounts for 60-75% of the total pore volume of the catalyst.
4. The catalyst according to claim 1, wherein The average pore size of the catalyst is 8-12 nm.
5. The catalyst according to claim 1, wherein The pore volume of the catalyst is 0.4-0.5 cm 3 / g.
6. The catalyst according to claim 1, wherein The water absorption rate of the alumina is greater than 0.9 mL / g, and the specific surface area is greater than 260 m 2 / g, the average pore size is greater than 8nm, and the pore distribution morphology is a unimodal pore distribution.
7. The catalyst according to claim 1, wherein In the alumina, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina.
8. The catalyst according to claim 7, wherein In the alumina, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 8% of the total pore volume of the alumina.
9. The catalyst according to claim 1, wherein In the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 4% of the total pore volume of the alumina.
10. The catalyst according to claim 9, wherein In the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 1% of the total pore volume of the alumina.
11. The catalyst according to any one of claims 1 to 10, wherein The molar ratio of Zi / Xi in the catalyst is 0.1-0.35:
1.
12. The catalyst according to claim 11, wherein The molar ratio of Zi / Xi in the catalyst is 0.2-0.35:
1.
13. The catalyst according to any one of claims 1 to 10, wherein The atomic concentration of the VIB group metal elements in the catalyst on the carrier surface is 2-6atom / nm 2 .
14. The catalyst according to claim 13, wherein The atomic concentration of the VIB group metal elements in the catalyst on the carrier surface is 3-4.5atom / nm 2 .
15. The catalyst according to any one of claims 1 to 10, wherein The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the catalyst is 0.2-0.
4.
16. The catalyst according to claim 15, wherein The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the catalyst is 0.2-0.
35.
17. The catalyst according to any one of claims 1 to 10, wherein The catalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds containing -OH, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds containing -OH to the metal element of Group VIII is 1-6.
18. The catalyst according to claim 17, wherein The molar ratio of the -OH-containing organic alcohol compound and / or carboxylic acid compound to the Group VIII metal element is 2-5.
19. The catalyst according to any one of claims 1 to 10, wherein The catalyst is in the shape of a cylinder, a three-leaf clover, a four-leaf clover, a butterfly, a honeycomb or other irregular shapes.
20. The catalyst according to any one of claims 1 to 10, wherein The equivalent diameter of the catalyst is 0.5-1.8 mm.
21. The catalyst according to claim 20, wherein The equivalent diameter of the catalyst is 0.8-1.6 mm.
22. A method for preparing a hydrogenation catalyst suitable for a high temperature section according to any one of claims 1 to 21, the method comprising: The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the alumina by an impregnation method, and then dried.
23. The preparation method according to claim 22, wherein: The impregnation method comprises: impregnating the aluminum oxide with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound containing -OH and / or a carboxylic acid compound.
24. The preparation method according to claim 23, wherein: The -OH-containing organic alcohol compound and / or carboxylic acid compound, Group VIII metal precursor, and Group VIB metal precursor are added to an aqueous solution of a phosphorus-containing compound to provide the impregnation solution.
25. The preparation method according to claim 22, wherein: The drying conditions include: temperature of 80-200° C. and time of 1-10 h.
26. Use of the hydrogenation catalyst suitable for high temperature section according to any one of claims 1 to 21 in a hydrodesulfurization reaction.
27. A hydrodesulfurization method, the method comprising: Under hydrodesulfurization conditions, the distillate oil is contacted with the catalyst for reaction, wherein the catalyst is the hydrogenation catalyst suitable for the high temperature section as described in any one of claims 1 to 21.
28. The hydrodesulfurization method according to claim 27, wherein: The conditions of the hydrodesulfurization include: pressure of 3-14 MPa, temperature of 350-410°C, volume space velocity of 0.5-10 hours -1 , the volume ratio of hydrogen to oil is 200-1000:
1.
29. The hydrodesulfurization method according to claim 28, wherein: The conditions for the hydrodesulfurization include: a temperature of 360-400°C.
Citation Information
Patent Citations
Diesel oil hydrorefining catalyst, and preparation method and applications thereof
CN108452843A
Hydrorefining catalyst and preparation method thereof
CN109692712A
Supported hydrogenation catalyst and preparation method thereof
CN111250103A
Hydrofining catalyst, and preparation method and application thereof
CN111558377A
Hydrodesulfurization catalyst, sulphur state hydrodesulfurization catalyst and their preparation methods
CN107961773A