A pure phase cobalt carbide nanomaterial and its preparation method and photothermal catalytic application

Pure-phase cobalt carbide nanomaterials are prepared by carbide cobalt-based Prussian blue analogues in a CO2/H2 reducing atmosphere, which solves the problems of harsh conditions and low yield of existing cobalt carbide synthesis methods, and can be used under photothermal catalytic conditions. It achieves efficient carbon dioxide hydrogenation activity, reduces costs, and promotes the industrial application and photothermal catalytic performance of cobalt carbide.

CN116040691BActive Publication Date: 2024-10-15SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211557812.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-10-15
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

Existing cobalt carbide synthesis methods have problems such as harsh experimental conditions, low yields, and formation of by-products, which hinder their large-scale production and industrial application. In addition, traditional photocatalysts have high costs and insufficient catalytic activity.

Method used

The cobalt-based Prussian blue analogue Co-PBA is used as a precursor, carbonized in a mixed reducing atmosphere of CO2/H2, to prepare pure phase cobalt carbide nanomaterials, and applied under photothermal catalytic conditions to improve carbon dioxide hydrogenation activity.

Benefits of technology

It achieves macro-scale preparation and mass production of cobalt carbide, reduces costs, improves catalytic performance, avoids excessive energy consumption at high temperatures and high pressures, and shows better catalytic performance than traditional platinum group noble metal-based catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116040691B_ABST
    Figure CN116040691B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of nanomaterial preparation, and specifically relates to a pure phase cobalt carbide nanomaterial, a preparation method thereof, and a photothermal catalytic application. The method of the present invention is simple, the conditions are mild, the product is pure, and a cobalt-based Prussian blue analog (Co-PBA) is used as a precursor, and carbonization is carried out in a mixed reducing atmosphere of CO2 / H2 to prepare pure phase cobalt carbide, which can be applied to the preparation of mass-produced cobalt carbide powder materials. In addition, since the cobalt carbide material has excellent light absorption ability, photothermal conversion ability, and excellent activation ability for reactants as a catalyst, light can be efficiently utilized, and therefore, it exhibits carbon dioxide hydrogenation activity superior to traditional platinum group noble metal-based catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of nano material preparation, and specifically relates to a pure phase cobalt carbide nano material and a preparation method and photothermal catalytic application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Transition metal carbides (TMCs) are a common type of interstitial alloys, which can be simply understood as periodically inserting carbon atoms into the atomic lattice of transition metals. Due to the introduction of carbon atoms, the electronic properties of TMCs can be adjusted by hybridization between the s and p orbitals of alloying carbon and the d orbitals of the host metal, so that TMCs exhibit surface properties similar to those of platinum group noble metals. As early as 1973, Levy, RB and Boudart, M. discovered that tungsten carbide exhibited catalytic behavior similar to that of the noble metal Pt in surface catalysis. At present, due to the unique electronic structure and surface properties, some common transition metal carbides, such as Mo 2 C,Ti 3 C 2 (MXenes), Nb 3 C 2 ,VC,WC,Fe 5 C 2 It has been widely reported to be used in various fields.

[0004] Cobalt carbide (Co 2 As a potential replacement material for Pt noble metals, cobalt carbide has been widely reported in the field of catalysis, especially in the Fischer-Tropsch reaction involving synthesis gas. In the early days, cobalt carbide was generally considered to be a sign of the deactivation of cobalt-based catalysts in the Fischer-Tropsch synthesis reaction and a by-product formed during the catalytic process. It was not until 2016 that Sun Yuhan's team at the Chinese Academy of Sciences discovered that Co 2 C as an active site in CoMn catalyst can efficiently realize the catalytic conversion from synthesis gas to olefins, which gives new insights into the role of cobalt carbide in catalytic reactions. At the same time, compared with precious metal catalysts, it is cheap. At present, cobalt carbide has shown good application potential in reverse water gas reaction (RWGS), electrocatalytic hydrogen production, epoxy addition reaction, etc. Cobalt carbide-based materials themselves have good stability and excellent magnetic properties. They have high coercivity at room temperature and are expected to become a substitute for rare earth magnets.

[0005] At present, the methods reported for synthesizing cobalt carbide are as follows: (1) high-temperature wet chemical method, which is mainly obtained by high-temperature pyrolysis of carbonyl cobalt compounds in an organic alcohol / amine medium under the protection of inert gas. This method is complicated to operate and has high requirements for experimental conditions. At the same time, the reactants are generally toxic; (2) programmed temperature carbonization reduction method, which is mainly obtained by carbonizing cobalt metal or cobalt oxide in a carbonizing atmosphere under high temperature conditions, in which the carbonizing reduction atmosphere is CO / H 2 (3) Laser etching, which is a typical method that often requires a multi-step carbonization process at high temperature; (4) Laser etching, which is mainly carried out on specific equipment under high vacuum conditions using metallic cobalt and carbon-rich precursors as reactants. In addition, there are a small number of reports on the synthesis of cobalt carbide by physical vapor deposition and atomic layer deposition. However, the above-mentioned methods and technologies have problems such as harsh experimental conditions, low yields and the formation of by-products, and are not very practical, which seriously hinders the development of the basic material properties and multiple application potential of cobalt carbide. However, looking at the research progress at home and abroad, there is currently no report on the controllable large-scale production of cobalt carbide.

[0006] Therefore, it is very necessary to establish a new synthesis method for large-scale production of single-phase cobalt carbide nanomaterials to explore the prospect of its substitution for precious metals. The present invention proposes a mild single-phase orthorhombic phase cobalt carbide powder nanomaterial preparation method, which has simple preparation conditions, safe process, and pure product, and can be applied to the large-scale preparation of cobalt carbide, which plays an important guiding role in promoting the industrial application of cobalt carbide nanomaterials.

[0007] CO mitigation 2 The impact of emissions has become one of the urgent problems that modern society needs to solve. 2 In emission reduction technology, light-heat coupling catalysis of CO 2 Hydrogenation can convert CO to 2 Converting it into high value-added chemicals is an effective way to alleviate environmental pollution and energy crisis. Studies have shown that the current mainstream photocatalysts are mainly precious metal-loaded catalysts, which are expensive and the catalytic activity still cannot meet the actual requirements of industry. Using cobalt carbide as a substitute for precious metal-based catalysts to achieve efficient light-heat coupled catalysis of carbon dioxide is of great significance to the equivalent reduction of photocatalysts at this stage. Summary of the invention

[0008] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a pure phase cobalt carbide nanomaterial and its preparation method and photothermal catalytic application. The method of the present invention is simple, mild and has a pure product. It uses cobalt-based Prussian blue analogue (Co-PBA) as a precursor and reacts with CO 2 / H 2The carbonization is carried out in a mixed reducing atmosphere to prepare pure phase cobalt carbide, which can be applied to the preparation of mass-produced cobalt carbide powder materials. In addition, since cobalt carbide materials as catalysts have excellent light absorption ability, photothermal conversion ability and excellent activation ability for reactants, they can efficiently utilize light, thus showing better carbon dioxide hydrogenation activity than traditional platinum group precious metal-based catalysts.

[0009] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing a pure phase cobalt carbide nanomaterial, comprising the following steps:

[0011] S1. Dissolving a cobalt salt and potassium cobalt cyanide in deionized water to obtain a cobalt salt solution and a potassium cobalt cyanide solution, respectively, mixing the cobalt salt solution and the potassium cobalt cyanide solution, standing, centrifuging, washing, drying, and grinding to obtain Co-PBA;

[0012] S2. Carbonizing and calcining Co-PBA in a reducing atmosphere to obtain pure phase cobalt carbide nanomaterials.

[0013] In a second aspect, the present invention provides a pure phase cobalt carbide nanomaterial, which is obtained by the above-mentioned preparation method of the pure phase cobalt carbide nanomaterial.

[0014] In a third aspect, the present invention provides the use of the above-mentioned pure phase cobalt carbide nanomaterial in photothermal catalytic carbon dioxide hydrogenation.

[0015] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:

[0016] (1) The preparation method provided by the present invention has a simple process, mild conditions, low cost, and pure products, and is suitable for the macro-preparation and batch production of pure phase cobalt carbide powder materials;

[0017] (2) The present invention uses pure phase cobalt carbide as a catalyst to achieve efficient light-heat coupled catalytic CO conversion under mild conditions. 2 Hydrogenation greatly avoids excessive energy consumption caused by high temperature and high pressure of traditional thermal catalytic reactions;

[0018] (3) Compared with traditional platinum group precious metal-based catalysts, cobalt carbide achieves better catalytic performance. As a powerful substitute for precious metals, it greatly reduces costs and helps to achieve industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0020] Figure 1 is an X-ray diffraction (XRD) diagram of the pure phase cobalt carbide nanomaterial obtained in Example 1 of the present invention;

[0021] Figure 2 is a scanning electron microscope (TEM) image of the pure phase cobalt carbide nanomaterial obtained in Example 1 of the present invention;

[0022] Figure 3 This is a surface scanning energy spectrum (Mapping) of the pure phase cobalt carbide nanomaterial obtained in Example 1 of the present invention;

[0023] Figure 4 This is the XRD diagram of the pure phase cobalt carbide nanomaterial obtained in Example 2 of the present invention;

[0024] Figure 5 This is the XRD diagram of the pure phase cobalt carbide nanomaterial obtained in Example 3 of the present invention;

[0025] Figure 6 It is a pure phase cobalt carbide nanomaterial and traditional platinum group noble metal-based catalyst that is photo-thermal coupled to catalytic CO 2 Comparison of product production rates of hydrogenation. DETAILED DESCRIPTION

[0026] A first typical embodiment of the present invention is a method for preparing a pure phase cobalt carbide nanomaterial, comprising the following steps:

[0027] S1. Dissolving a cobalt salt and potassium cobalt cyanide in deionized water to obtain a cobalt salt solution and a potassium cobalt cyanide solution, respectively, mixing the cobalt salt solution and the potassium cobalt cyanide solution, standing, centrifuging, washing, drying, and grinding to obtain Co-PBA;

[0028] S2. Carbonizing and calcining Co-PBA in a reducing atmosphere to obtain pure phase cobalt carbide nanomaterials.

[0029] In one or more examples of this implementation mode, the cobalt salt is one or more of cobalt nitrate, cobalt acetate, and cobalt chloride.

[0030] In one or more examples of this embodiment, the molar ratio of the cobalt salt to potassium cobalt cyanide is 0.5-3:1.

[0031] In one or more examples of this implementation, the mixing process is to slowly drop the cobalt salt solution into the potassium cobalt cyanide solution at a uniform speed under room temperature and stirring.

[0032] In one or more examples of this embodiment, the standing time is 0-96h, and the standing temperature is room temperature;

[0033] The centrifugal speed is 5000-10000 rpm, and the centrifugal time is 5-10 min;

[0034] The cleaning reagents were deionized water and ethanol;

[0035] The drying temperature is 50-150°C and the drying time is 2-48h.

[0036] In one or more embodiments of this embodiment, the reducing atmosphere is H 2 and CO 2 Mixed gas, H 2 and CO 2 The volume ratio is 1:4-4:1.

[0037] In one or more examples of this embodiment, the temperature of the carbonization roasting is 230-330° C., and the time is 5-15 hours.

[0038] A second typical embodiment of the present invention is a pure phase cobalt carbide nanomaterial, which is obtained by the above-mentioned preparation method of the pure phase cobalt carbide nanomaterial.

[0039] A third typical implementation of the present invention is the use of the above-mentioned pure phase cobalt carbide nanomaterial in photothermal catalytic carbon dioxide hydrogenation.

[0040] In one or more examples of this embodiment, the catalytic conditions are: the light source is a xenon lamp with a wavelength of 420-780nm and a light intensity of 2W·cm -2 , CO 2 The flow rate is 3-5 mL / min, H 2 The flow rate is 12-20 mL / min, the reaction temperature is 100-300° C., the reaction apparatus is a gas phase flow reactor, and the catalyst dosage is 20-40 mg.

[0041] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.

[0042] Example 1

[0043] (1) Weigh 0.75 mmol of cobalt acetate and 0.5 mmol of potassium cobalt cyanide to prepare a solution, add 100 mL of deionized water to each solution, and stir to fully dissolve them.

[0044] (2) Add the prepared cobalt acetate solution dropwise into the potassium cobalt cyanide solution and continue stirring for 10 minutes after the addition.

[0045] (3) The obtained pink suspension was allowed to stand at room temperature for 24 h, and the obtained Co-PBA was centrifuged at 7000 rpm for 5 min, washed twice with deionized water, then washed twice with anhydrous ethanol, dried at 60°C for 24 h, and then ground.

[0046] (4) Place the ground Co-PBA in H 2 :CO 2 =4:1 mixed reducing atmosphere, carbonization calcination is carried out at 250°C, the heat preservation time is 5h, and the material is taken out after carbonization to obtain pure phase cobalt carbide nanomaterials.

[0047] like Figure 1 As shown in the figure, it can be seen that the diffraction peak position of the material is consistent with the standard Co 2 The main peak positions of C (PDF#72-1369) coincide with each other, indicating that the prepared sample is a single orthorhombic phase of Co 2 C material. Morphology Figure 2 As shown, it can be seen that the pure phase cobalt carbide nanomaterial presents a spherical nanoparticle morphology, and the particle size distribution is between 10-30 nanometers. Figure 3 As shown, the mapping diagram shows the uniform distribution of carbon and cobalt elements in the pure phase cobalt carbide nanomaterials.

[0048] Example 2

[0049] 1) Weigh 7.5 mmol of cobalt acetate and 5.0 mmol of potassium cobalt cyanide to prepare a solution, add 100 mL of deionized water respectively, and stir to fully dissolve.

[0050] (2) The prepared cobalt acetate solution was instantly added dropwise to the potassium cobalt cyanide solution, and stirring was continued for 10 minutes after the addition was completed.

[0051] (3) The obtained pink suspension was allowed to stand at room temperature for 24 h, and the obtained Co-PBA was centrifuged at 7000 rpm for 5 min, washed twice with deionized water, then washed twice with anhydrous ethanol, dried at 60°C for 24 h, and then ground.

[0052] (4) Place the ground Co-PBA in H 2 :CO 2 =4:1 mixed reducing atmosphere, carbonization calcination is carried out at 230°C, the heat preservation time is 10h, and after carbonization is completed, it is taken out to obtain a pure phase cobalt carbide nanomaterial.

[0053] like Figure 4 As shown, it can be seen from the XRD diagram that changing the amount of raw materials will not affect the crystal form and type of the cobalt carbide product.

[0054] Example 3

[0055] (1) Weigh 0.75 mmol of cobalt acetate and 0.5 mmol of potassium cobalt cyanide to prepare a solution, add 100 mL of deionized water to each solution, and stir to fully dissolve them.

[0056] (2) Add the prepared cobalt acetate solution dropwise into the potassium cobalt cyanide solution, and continue stirring for 10 minutes after the addition is completed.

[0057] (3) The obtained pink suspension was allowed to stand at room temperature for 24 h, and the obtained Co-PBA was centrifuged at 7000 rpm for 5 min, washed twice with deionized water, then washed twice with anhydrous ethanol, dried at 60°C for 24 h, and then ground.

[0058] (4) Place the ground Co-PBA in H 2 :CO 2 =1:1 mixed reducing atmosphere, carbonization calcination is carried out at 300°C, the heat preservation time is 5h, and the material is taken out after carbonization to obtain pure phase cobalt carbide nanomaterials.

[0059] like Figure 5 As shown in the XRD diagram, it can be seen that adjusting H 2 :CO 2 With the increase of gas ratio and carbonization temperature, the position of XRD diffraction peak remains unchanged and the product is still a single-phase cobalt carbide material.

[0060] Example 4

[0061] (1) Weigh 0.75 mmol of cobalt acetate and 0.5 mmol of potassium cobalt cyanide to prepare a solution, add 100 mL of deionized water to each solution, and stir to fully dissolve them.

[0062] (2) Add the prepared cobalt acetate solution dropwise into the potassium cobalt cyanide solution, and continue stirring for 10 minutes after the addition is completed.

[0063] (3) The obtained pink suspension was allowed to stand at room temperature for 12 h, and the obtained Co-PBA was centrifuged at 10,000 rpm for 5 min, washed twice with deionized water, then washed twice with anhydrous ethanol, dried at 70°C for 24 h, and then ground.

[0064] (4) Place the ground Co-PBA in H 2 :CO 2 =1:4 mixed reducing atmosphere, carbonization roasting is carried out at 300°C, the heat preservation time is 5h, and after carbonization is completed, it is taken out to obtain a pure phase cobalt carbide nanomaterial.

[0065] Experimental Example 1

[0066] Pt / Al 2 O 3 Preparation:

[0067] Add 2 mL of H 2 PtCl6 Solution (Pt: 1 mg / mL), 200 mg Al 2 O 3 Disperse into 100 mL of deionized water and stir for 2 hours.

[0068] (2) Then, under stirring, excess NaBH 4 The solution (0.1 mol / L, 5 mL) was quickly added to the suspension and stirred for 2 hours, after which the Pt / Al 2 O 3 for further use.

[0069] Ru / Al 2 O 3 Preparation:

[0070] Add 2 mL of H 2 RuCl 5 Solution (Ru: 1 mg / mL), 200 mg Al 2 O 3 Disperse into 100 mL of deionized water and stir for 2 hours.

[0071] (2) Then, under stirring, excess NaBH 4 The solution (0.1 mol / L, 5 mL) was quickly added to the suspension and stirring was continued for 2 h, after which the sample was washed and dried and collected for further use.

[0072] Photo-thermal coupled catalysis of CO 2 Hydrogenation test:

[0073] CO 2 The hydrogenation experiment was carried out in a photothermal catalytic microreactor system, and the reaction system was a flow system. The catalytic conditions were: the light source was a xenon lamp with a wavelength of 420-780nm and a light intensity of 2W·cm -2 , CO 2 The flow rate was 4 mL / min, H 2 The flow rate was 16 mL / min, and the reaction temperature was 100-250° C. 30 mg of the pure phase cobalt carbide nanomaterial (Co 2 C) Pt / Al 2 O 3 、Ru / Al 2 O 3 As a catalyst, it was fully mixed with 1.25 g of quartz sand and placed in a transparent quartz tube. The quartz tube was placed in a heating furnace and CO was introduced. 2 and H 2 , turn on the light source, and obtain CO through the online connected gas chromatograph 2 and product concentration data, and then compare the photothermal catalytic CO2 Hydrogenation activity. Figure 6 As shown, the bar graph from left to right is Pt / Al 2 O 3 、Ru / Al 2 O 3 , the pure phase cobalt carbide nanomaterial prepared in Example 1 is compared with the traditional Pt / Al 2 O 3 , Ru / Al 2 O 3 The catalyst, phase-pure cobalt carbide nanomaterials, exhibited higher photothermal effect, carbon dioxide conversion rate and product yield.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a pure phase cobalt carbide nanomaterial, characterized in that: The following steps are involved: S1. Dissolving a cobalt salt and potassium cobalt cyanide in deionized water to obtain a cobalt salt solution and a potassium cobalt cyanide solution, respectively, mixing the cobalt salt solution and the potassium cobalt cyanide solution, standing, centrifuging, washing, drying, and grinding to obtain Co-PBA; S2, carbonizing and calcining Co-PBA in a reducing atmosphere to obtain a pure phase cobalt carbide nanomaterial; The reducing atmosphere is a mixed gas of H2 and CO2, and the volume ratio of H2 to CO2 is 1:4-4:1; The carbonization calcination temperature is 230-330°C and the time is 5-15 h; The cobalt salt is one or more of cobalt nitrate, cobalt acetate and cobalt chloride; The molar ratio of the cobalt salt to potassium cobalt cyanide is 0.5-3:

1.

2. The method for preparing the pure phase cobalt carbide nanomaterial according to claim 1, characterized in that: The mixing process is to slowly drop the cobalt salt solution into the potassium cobalt cyanide solution at a uniform speed under room temperature and stirring.

3. The method for preparing the pure phase cobalt carbide nanomaterial according to claim 1, characterized in that: The standing time is 0-96h, and the standing temperature is room temperature; The centrifugal speed is 5000-10000 rpm, and the centrifugal time is 5-10 min; The cleaning reagents were deionized water and ethanol; The drying temperature is 50-150 ℃ and the drying time is 2-48 h.

4. Application of the pure phase cobalt carbide nanomaterial prepared by the preparation method according to claim 1 in photothermal catalytic carbon dioxide hydrogenation.

5. The use according to claim 4, characterized in that The catalytic conditions are as follows: the light source is a xenon lamp with a wavelength of 420-780 nm and a light intensity of 2 W·cm -2 , CO2 flow rate is 3-5 mL / min, H2 flow rate is 12-20 mL / min, reaction temperature is 100-300 ℃, reaction apparatus is a gas phase flow reactor, and catalyst dosage is 20-40 mg.