A cadmium ion detection material and its preparation method and application
By adding a chromogenic monomer and a specific dispersant to the cadmium ion detection material, and using the suspension polymerization method to prepare the cadmium ion detection material, the problems of high detection limit and low accuracy of cadmium ion detection in the existing technology are solved, and the High sensitivity, rapid and accurate detection of cadmium ions, with a detection limit of 0.02mg/L.
Patent Information
- Application Number
- CN202310063020.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-18
AI Technical Summary
Existing cadmium ion rapid detection products have high detection limits, low accuracy, and are susceptible to interference, making it difficult to quickly and accurately detect trace amounts of cadmium ions on site.
Using the ion imprinting polymer preparation method, adding chromogenic monomers and preparing cadmium ion detection materials through suspension polymerization, combined with specific dispersants to improve anti-interference ability and color sensitivity, lower the detection limit to 0.02mg/L.
It achieves high sensitivity, specific identification and rapid color detection of cadmium ions. The color detection results are accurate, the anti-interference ability is strong, the detection limit reaches 0.02mg/L, and it is suitable for on-site rapid detection.
Smart Images

Figure BDA0004061505270000081 
Figure BDA0004061505270000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of rapid heavy metal detection, and more specifically, to a cadmium ion detection material and a preparation method and application thereof. Background Art
[0002] With the development of industry, more and more heavy metals are released into the environment, which is an important part of environmental pollutants. Heavy metals have many characteristics such as high toxicity, non-biodegradability, and easy migration. Among them, cadmium is a highly carcinogenic metal that can cause toxic reactions even at low concentrations, causing lesions in human skin, bones, and teeth. In view of the serious harm that cadmium can cause to the human body, it is necessary to accurately detect the cadmium ion content in the environment.
[0003] At present, the detection methods for cadmium ions are relatively mature, and the commonly used ones are: atomic absorption spectroscopy, atomic emission spectroscopy, atomic fluorescence spectroscopy, inductively coupled plasma emission spectroscopy, etc. These technologies are highly sensitive, but the instruments are expensive and complicated to operate. They can only be used for laboratory detection and analysis, and sometimes require complex and time-consuming pre-treatment. Commercially available cadmium ion rapid detection products are greatly affected by interference from other ions and have low accuracy. Therefore, it is very necessary to further develop on-site rapid detection materials with strong trace cadmium ion enrichment ability, good selectivity, no need for complex pre-treatment, and reliable results.
[0004] Ion imprinting technology is a technology that selects target ions as templates to synthesize materials with specific adsorption functions for target ions, which are used for selective enrichment and separation of target ions. The basic principle is to select functional monomers with certain binding ability to target ions, polymerize under the action of crosslinking agents and initiators, and elute the target ions to obtain three-dimensional hole polymers with specific recognition ability for target ions, namely ion imprinted polymers. The current synthesis method of ion imprinted materials is relatively mature, and the materials synthesized by suspension polymerization have a large specific surface area, good sedimentation properties and high mechanical strength. However, most of the existing technologies use ion imprinting technology to selectively enrich, adsorb and separate target ions, and few are used for target ion detection.
[0005] The prior art discloses a paper-based ion-imprinted composite material, in which an ion-imprinted polymer is prepared by modifying the ion-imprinted material on the surface of a paper material. The ion-imprinted polymer can quickly detect cadmium ions through conventional color development technology. However, specifically, when detecting the cadmium ion content, the composite material uses a splash color development reagent. The detection effect is affected by the splash amount, the accuracy is poor, and the detection limit is only 1 ng / mL, i.e., 1 mg / L, that is, the sensitivity still needs to be improved. Summary of the invention
[0006] In order to solve the problems in the prior art that cadmium ion rapid detection products have high detection limits but low accuracy and are susceptible to interference, the present invention provides a method for preparing a cadmium ion detection material. The cadmium ion detection material is an ion imprinted polymer, and a color-developing monomer is added during the preparation process. Therefore, the ion imprinted polymer has specific recognition ability for cadmium ions and strong anti-interference ability, and can quickly develop color after identifying the cadmium ions. In addition, the present invention also improves the preparation process of the ion imprinted polymer by adopting a suspension polymerization method and adding a dispersant during the preparation process, so that the detection limit of the material provided by the present invention for cadmium ions is finally reduced to 0.02 mg / L.
[0007] Another object of the present invention is to provide a cadmium ion detection material.
[0008] Another object of the present invention is to provide an application of a cadmium ion detection material.
[0009] Another object of the present invention is to provide a method for detecting cadmium ions.
[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0011] A method for preparing a cadmium ion detection material specifically comprises the following steps:
[0012] S1. dissolving the cadmium salt, the color-developing monomer and the comonomer in an organic solvent at a molar ratio of 1:(1-3):(0-4), adjusting the pH to an alkaline solution, sonicating until completely dissolved, and prepolymerizing by shaking to prepare a solution 1;
[0013] S2. Preparation of a polymerizing agent solution: dissolving a crosslinking agent and an initiator in an organic solvent to obtain a polymerizing agent solution;
[0014] S3. Preparation of a dispersant solution: mixing a sodium dodecylbenzene sulfonate solution and a Triton X-100 solution to obtain a dispersant solution, wherein the mass percentage concentrations of sodium dodecylbenzene sulfonate and Triton X-100 are 1%-5% and 5%-10%, respectively;
[0015] S4. Add the above obtained polymerizing agent and dispersant solution to solution 1, react by shaking at 65-75° C. for 9 to 12 hours to obtain a polymerized product, and wash to obtain a cadmium ion detection material;
[0016] The color-developing monomer in step S1 is a triazene reagent.
[0017] The present invention adds a chromogenic monomer in the step S1 of preparing the ion-imprinted polymer, so as to make the ion-imprinted polymer contain a part for color development, combine the specific recognition ability of the ion-imprinted polymer with the detection ability of the color development technology, so that the prepared ion-imprinted polymer has a specific recognition ability for cadmium ions and can quickly develop color after recognizing the cadmium ions, can be used to quickly detect the existence and content of cadmium ions, and has strong anti-interference ability; at the same time, the chromogenic monomer is used to prepare the ion-imprinted polymer, so that the cadmium ion detection material prepared by the present invention has a color development detection function. If the chromogenic monomer is added after the preparation of the ion-imprinted material is completed, the chromogenic monomer only exists on the surface of the material in a simple attached form, and is easily separated from the surface of the material after the water sample is subsequently added, so that the material does not have a color development detection function.
[0018] The present invention adopts suspension polymerization method, and reacts between reactants by shaking, and then prepares ion imprinted polymer, and the material sedimentation performance of the synthesized material is good. When the water sample has a certain chromaticity, there is a large error in identifying the color development of the material that is not convenient for solid-liquid separation, and when the material sedimentation performance is good, the supernatant can be poured after the color development is complete, and then more accurate color development identification is performed; at present, most of the water samples that are polluted and need to determine the cadmium ion content have a certain chromaticity, so the suspension polymerization method is used to prepare the cadmium ion detection material in the present invention, and it is ensured that the detection limit of the prepared cadmium ion detection material for cadmium ions can be as low as 0.02mg / L.
[0019] The comonomer in step S1 is not necessarily added. When the molar ratio of the comonomer to the other two reactants in step S1 is 0, although the anti-interference of the prepared cadmium ion detection material is slightly weak, it is still improved relative to the prior art, and the detection limit of cadmium ions is still 0.02mg / L. The specific reason may be that the comonomer plays the role of improving the ion-imprinted polymer structure in the present invention. The reason why the cadmium ion detection material provided by the present invention can specifically identify cadmium ions is that it can be combined with the effect of hydrogen bonds when encountering cadmium ions, but the three-dimensional holes inside the cadmium ion detection material can hinder the combination of other ions with themselves to a certain extent, forming a specific adsorption effect. When the comonomer is lacking in the polymerization system, the three-dimensional hole structure formed inside the material may not be clear enough, but the detection sensitivity for cadmium ions is still high.
[0020] The molar ratio of the cadmium salt, the color-developing monomer and the comonomer in step S1 is limited to 1:(1-3):(0-4), and in step S3, a dispersant is added to the system and its type is limited to sodium dodecylbenzene sulfonate and Triton X-100, and its mass percentage concentration is limited to 1%-5% and 5%-10%, respectively. The specific technical effect achieved is that the droplets have the best stability during the suspension polymerization process, thereby improving the effect of the suspension polymerization, and finally enhancing the anti-interference ability of the material and improving the color sensitivity. The ratio between the cadmium salt and the functional monomer and the dispersant are defined as above, and the detection limit of the present invention for cadmium ions can be as low as 0.02mg / L.
[0021] The color-developing monomer in step S1 is a triazene reagent. The color-developing reaction between triazene compounds and cadmium ions is very sensitive. Only by using such a sensitive color-developing monomer to participate in color-developing detection can the detection limit of cadmium ion detection provided by the cadmium ion detection material of the present invention be achieved.
[0022] Preferably, the shaking prepolymerization time in step S1 is 2 to 3 hours.
[0023] Before polymerization, prepolymerization occurs between the reactants in order to achieve a better polymerization effect. When the polymerization effect of the ion-imprinted polymer is better, its structure is clearer and it has a higher anti-interference ability for the detection of cadmium ions.
[0024] Preferably, the organic solvent in step S1 is dimethyl sulfoxide (DMSO).
[0025] Preferably, the color-developing monomer in step S1 is arbitrarily selected from one or more of p-chlorophenyldiazoaminoazobenzene, Dadan Yellow, o-carboxyphenyldiazoaminoazobenzene and p-nitrobenzenediazoaminoazobenzene.
[0026] Preferably, the comonomer in step S1 is arbitrarily selected from one or more of methacrylic acid, L-cysteine, 4-vinylpyridine and allylthiourea.
[0027] Preferably, the prepolymerization in step S1 is carried out at room temperature.
[0028] Preferably, in step S2, the ratio of the crosslinking agent and the initiator to the cadmium salt is (120-200):(1.5-4.5):1.
[0029] Preferably, the organic solvent in step S2 is toluene.
[0030] Preferably, in step S2, the cross-linking agent is ethylene glycol dimethacrylate.
[0031] When the cross-linking agent used is ethylene glycol dimethacrylate, the cadmium ion detection material prepared by the present invention can have stronger anti-interference ability. The specific reason may be that the reaction between ethylene glycol dimethacrylate and triazene-type color-developing monomers and copolymers can form more stable three-dimensional holes that are adapted to the cadmium ion structure.
[0032] Preferably, the initiator in step S2 is azobisisobutyronitrile.
[0033] Preferably, in step S4, the volume ratio of the polymerizing agent, the dispersant and the solution 1 is 2:(5-8):(4-7).
[0034] Preferably, in step S4, nitrogen is introduced during the reaction to remove oxygen.
[0035] The oxygen in the system will have a certain inhibitory effect on the polymerization reaction. The introduction of nitrogen to deoxygenate the material can make the polymerization reaction proceed more smoothly.
[0036] Preferably, the specific operation of washing in step S4 is to wash the obtained polymer product with methanol to wash away the unreacted reagent, then elute with HCl solution to remove the cadmium ion template, elute several times until no cadmium ions can be detected in the supernatant using an atomic absorption spectrometer, and finally wash with ultrapure water several times and dry.
[0037] More preferably, the concentration of the HCl solution used to elute the cadmium ion template in step S4 is 0.01 mol / L.
[0038] The present invention also protects a cadmium ion detection material prepared by the preparation method.
[0039] The present invention also protects an application of the cadmium ion detection material.
[0040] The present invention also protects a cadmium ion detection method using the cadmium ion detection material.
[0041] The cadmium ion detection method using the above-mentioned cadmium ion detection material specifically comprises the following steps:
[0042] S6. Prepare standard color scale of cadmium ions;
[0043] S7. Adjust the pH value of the solution sample containing cadmium ions to be tested, add the cadmium ion detection material to the liquid sample to be tested, add the surfactant solution, shake, let stand, and wait for the material to precipitate;
[0044] S8. Compare the color displayed by the cadmium ion rapid colorimetric detection ion imprinting material with the cadmium ion standard color scale to perform a semi-quantitative analysis of the cadmium ions in the liquid sample.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] The present invention directly adds color-developing monomers to participate in polymerization during the preparation process of the cadmium ion imprinted polymer. The prepared cadmium ion detection material has the properties of the ion imprinted material and has specific recognition ability for cadmium ions and strong anti-interference ability. The part formed by polymerization of the color-developing monomers can react with cadmium ions quickly and sensitively. At the same time, the present invention adopts a suspension polymerization method to prepare the cadmium ion detection material, and adds a dispersant of a specific type and concentration during the preparation process. Therefore, the cadmium ion detection material provided by the present invention has a detection limit for cadmium ions as low as 0.02 mg / L. DETAILED DESCRIPTION
[0047] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0048] Example 1
[0049] A method for preparing a cadmium ion detection material specifically comprises the following steps:
[0050] S1. Prepare solution 1: using p-nitrobenzenediazoaminoazobenzene as the color-developing monomer, dissolve CdCl2 powder and the color-developing monomer in DMSO at a molar ratio of 1:2, the CdCl2 concentration in the solution is 3.3 mol / L, add an appropriate amount of sodium hydroxide solution to make it alkaline, sonicate until completely dissolved, and prepolymerize on a shaker at room temperature for 3 hours;
[0051] S2. Preparation of polymerization agent: 16 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.04 g of initiator azobisisobutyronitrile were dissolved in 10 mL of toluene, and the molar ratio of crosslinking agent to initiator in the obtained polymerization agent was 66.67:1;
[0052] S3. Preparation of dispersant: Prepare 50 mL of a mixed solution of 1% and 8% by mass of sodium dodecylbenzene sulfonate and Triton X-100;
[0053] S4. Mix the prepared polymerizer, dispersant and solution 1 in a volume ratio of 1:3:3, introduce nitrogen to deoxygenate, and shake on a constant temperature shaker at 70°C for 12 hours to obtain a polymerization product; wash the polymerization product with methanol to remove unreacted functional monomers and cross-linking agents, and then elute with 0.01 mol / L HCl solution to remove the template cadmium ions until no cadmium ions can be detected in the supernatant; finally, wash with ultrapure water until neutral and then blow dry for 24 hours to obtain an ion imprinting material for on-site rapid colorimetric detection of cadmium ions.
[0054] Example 2
[0055] A method for preparing a cadmium ion detection material, which differs from Example 1 in that:
[0056] In step S1, the molar ratio of CdCl2 powder to color-developing monomer is 1:3.
[0057] Example 3
[0058] A method for preparing a cadmium ion detection material, which differs from Example 1 in that:
[0059] In step S1, the molar ratio of CdCl2 powder to the color-developing monomer is 1:1.
[0060] Example 4
[0061] A method for preparing a cadmium ion detection material, which differs from Example 1 in that:
[0062] In step S1, 4-vinylpyridine is added as a comonomer, and CdCl2, a chromogenic monomer and a comonomer are dissolved in DMSO at a molar ratio of 1:1:1;
[0063] In step S2, 20 mmol of a cross-linking agent and 0.05 g of an initiator are dissolved in 10 mL of toluene;
[0064] The solute and concentration of the dispersant solution prepared in step S3 are 1% sodium dodecylbenzene sulfonate and 10% Triton X-100 respectively;
[0065] In step S4, the prepared polymerizing agent, dispersant and solution 1 are mixed in a volume ratio of 2:7:6.
[0066] Example 5
[0067] A method for preparing a cadmium ion detection material, which differs from Example 1 in that:
[0068] In step S1, the molar ratio of CdCl2 powder, color-developing monomer and comonomer is 1:2:2.
[0069] Example 6
[0070] A method for preparing a cadmium ion detection material, which differs from Example 1 in that:
[0071] In step S1, the molar ratio of CdCl2 powder, color-developing monomer and comonomer is 1:1:4.
[0072] Example 7
[0073] A method for preparing a cadmium ion detection material, which differs from Example 1 in that:
[0074] The mass percentage concentration of sodium dodecylbenzene sulfonate in the dispersant in step S3 is 2%.
[0075] Example 8
[0076] A method for preparing a cadmium ion detection material, which differs from Example 1 in that:
[0077] In step S3, the mass percentage concentrations of sodium dodecylbenzene sulfonate and Triton X-100 in the dispersant are 5% and 5% respectively.
[0078] Example 9
[0079] A method for preparing a cadmium ion detection material, which differs from Example 1 in that:
[0080] The mass percentage concentration of Triton X-100 in the dispersant in step S3 is 10%.
[0081] Comparative Example 1
[0082] A method for preparing a cadmium ion imprinted material, which differs from Example 4 in that:
[0083] In step S1, no color-developing monomer is added;
[0084] In step S4, after the cadmium ion imprinting material is prepared, the color-developing monomer is mixed with the cadmium ion imprinting material.
[0085] Comparative Example 2
[0086] A method for preparing a cadmium ion imprinted material, which differs from Example 1 in that:
[0087] In step S1, the molar ratio of CdCl2 powder to color-developing monomer is 1:6.
[0088] Comparative Example 3
[0089] A method for preparing a cadmium ion imprinted material, which differs from Example 1 in that:
[0090] In step S1, the molar ratio of CdCl2 powder, color-developing monomer and comonomer is 1:2:8.
[0091] Comparative Example 4
[0092] A method for preparing a cadmium ion imprinted material, which differs from Example 1 in that:
[0093] In step S3, sodium dodecylbenzene sulfonate is not added to the dispersant.
[0094] Comparative Example 5
[0095] A method for preparing a cadmium ion imprinted material, which differs from Example 1 in that:
[0096] In step S3, no Triton X-100 is added to the dispersant.
[0097] Comparative Example 6
[0098] A method for preparing a cadmium ion imprinted material, which differs from Example 1 in that:
[0099] The mass percentage concentration of sodium dodecylbenzene sulfonate in the dispersant in step S3 is 10%.
[0100] Comparative Example 7
[0101] A method for preparing a cadmium ion imprinted material, which differs from Example 1 in that:
[0102] The mass percentage concentration of Triton X-100 in the dispersant in step S3 is 15%.
[0103] Performance Testing
[0104] The specific steps of using the cadmium ion detection material prepared by the present invention to detect the cadmium ion content are as follows:
[0105] S6. Prepare 0 mg / L, 0.02 mg / L, 0.05 mg / L, 0.07 mg / L, 0.1 mg / L, 0.3 mg / L, 0.5 mg / L cadmium ion solution, take 10 mL of each and place it in a 10 mL colorimetric tube, then add 0.01 g of the cadmium ion detection material prepared in Example 2, add 10% Triton X-100 solution, and add a suitable sodium hydroxide solution to adjust the pH to 11, shake and let stand for 5-10 min to obtain a cadmium ion standard color scale;
[0106] S7. The pH value of the solution sample containing cadmium ions is adjusted to 11, and then 0.01 g of cadmium ion detection material is added to 10 mL of liquid sample, and after adding the surfactant solution, it is shaken for 30 seconds and allowed to stand to wait for the material to precipitate;
[0107] S8. Compare the color displayed by the cadmium ion detection material with the standard color scale of cadmium ions, and conduct semi-quantitative analysis of cadmium ions in contaminated water samples.
[0108] The color development results of the cadmium ion detection material obtained in Example 2 were compared with the data measured by atomic absorption spectroscopy, and the results are shown in Table 1 below.
[0109] Prepare cadmium ion solutions of different concentrations, and perform the experiment according to step S7. The cadmium ion detection material used is the cadmium ion detection material prepared by the embodiment of the present invention and the comparative example. Compare the color development result of the obtained cadmium ion detection material with the cadmium ion standard color scale, and the result is shown in Table 2 below.
[0110] Table 1 Detection and analysis results of cadmium ion content in cadmium ion-containing water samples
[0111]
[0112] Table 2 Comparison of color development test results of the embodiment and the comparative example
[0113]
[0114] It can be seen from Table 1 that the cadmium ion detection material provided in Example 2 of the present invention has a color detection result for a specific concentration of cadmium ion solution that is basically consistent with the instrument measurement result, has high accuracy, and can maintain stable color detection results in three parallel experiments with good reproducibility.
[0115] It can be seen from Table 2 that the cadmium ion detection material provided in the embodiment of the present invention has a good detection effect for a cadmium ion solution with a concentration of 0.02 mg / L, that is, the detection limit of the cadmium ion detection material provided by the present invention can reach 0.02 mg / L; while the cadmium ion detection material prepared by the preparation method provided in the comparative example has a detection limit basically higher than 0.05 mg / L, and the preparation methods used in some comparative examples cannot prepare materials that can be used to detect the cadmium ion content, and even cannot successfully synthesize the cadmium ion detection material.
[0116] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a cadmium ion detection material, characterized in that: The specific steps include: S1. dissolving the cadmium salt, the color-developing monomer and the comonomer in an organic solvent at a molar ratio of 1:(1-3):(0-4), adjusting the pH to an alkaline solution, sonicating until completely dissolved, and prepolymerizing by shaking to prepare a solution 1; S2. Preparation of a polymerizing agent solution: dissolving a crosslinking agent and an initiator in an organic solvent to obtain a polymerizing agent solution; S3. Preparation of a dispersant solution: mixing a sodium dodecylbenzene sulfonate solution and a Triton X-100 solution to obtain a dispersant solution, wherein the mass percentage concentrations of sodium dodecylbenzene sulfonate and Triton X-100 in the dispersant solution are 1%-5% and 5%-10% respectively; S4. Add the polymerizing agent solution and dispersant solution obtained above to solution 1, react by shaking at 65-75° C. for 9 to 12 hours to obtain a polymerized product, and wash to obtain a cadmium ion detection material; The color-developing monomer in step S1 is arbitrarily selected from one or more of p-chlorophenyldiazoaminoazobenzene, Dadan Yellow, o-carboxyphenyldiazoaminoazobenzene and p-nitrobenzenediazoaminoazobenzene; In step S4, the volume ratio of the polymerizing agent solution, the dispersant solution and the solution 1 is 2:(5-8):(4-7).
2. The method for preparing a cadmium ion detection material according to claim 1, wherein: The comonomer in step S1 is arbitrarily selected from one of methacrylic acid, L-cysteine, 4-vinylpyridine and allylthiourea.
3. The method for preparing a cadmium ion detection material according to claim 1, wherein: The shaking prepolymerization time in step S1 is 2 to 3 hours.
4. The method for preparing a cadmium ion detection material according to claim 1, wherein The ratio of the cross-linking agent, the initiator and the cadmium salt in step S2 is (120-200): (1.5-4.5):
1.
5. The method for preparing the cadmium ion detection material according to claim 1, wherein The cross-linking agent in step S2 is ethylene glycol dimethacrylate.
6. A cadmium ion detection material, characterized in that: The cadmium ion detection material is prepared by the preparation method of the cadmium ion detection material according to any one of claims 1 to 5.
7. Use of the cadmium ion detection material according to claim 6 in detecting cadmium ion content for non-diagnostic purposes.
8. A method for detecting cadmium ions, characterized in that: The cadmium ion detection method is carried out using the cadmium ion detection material described in claim 6.