A high-strength heat shrinkable tube material, a high-strength heat shrinkable tube and its application
Through extrusion granulation and melt-kneading of vinyl triethoxysilane, ethylene-vinyl acetate copolymer and other materials, high-strength heat shrinkable sleeve materials are formed, which solves the problem of insufficient insulation in the prior art and realizes the The material has good heat shrinkage properties, tensile strength and flame retardancy, suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202211542797.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-02
AI Technical Summary
The existing heat shrinking materials have shortcomings in insulation properties, and it is difficult to meet the requirements of better heat shrinkability, tensile strength and flame retardancy at the same time.
Extrusion granulation and melt-kneading using vinyl triethoxysilane, ethylene-vinyl acetate copolymer, diisopropyl peroxide, modified copolymer and hydrotalcite slurry to form a high-strength heat shrinkable sleeve Materials, the thermal shrinkage, tensile strength and insulation of the material are improved by modifying the multi-chain mesh structure and three-dimensional network structure of the copolymer.
It realizes good heat shrinkability, high tensile strength, excellent flame retardancy and insulation of heat shrink sleeve materials, and is suitable for the protection of automotive industry, industrial equipment and electronic communication cable harnesses.
Smart Images

Figure BDA0003978479700000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a high-strength heat shrinkable tube material, a high-strength heat shrinkable tube and applications thereof. Background Art
[0002] Heat shrinkable materials are functional polymer materials made by mixing, molding, cross-linking, heating, expanding, cooling and finalizing rubber and plastic materials based on the principle of "elastic memory" of polymers. They usually have an incompletely compatible two-phase structure, which are called stationary phase and reversible phase, or hard segment and soft segment. Heat shrinkable materials are an important type of shape memory polymers. They belong to heat-driven shape memory polymers and are widely used in the automotive industry, power industry, medical equipment, packaging materials, pipeline transportation, military industry and other fields. Cross-linking is one of the prerequisites for the polymer memory effect. In order to make the polymer have shape memory function, it is necessary to add a crystalline phase to the amorphous phase interval formed by cross-linking. Materials with memory effect are mainly composed of stationary phase and reversible phase (crystalline phase) of the non-cross-linked part. When the cross-linked polymer is heated above the melting point Tm, the crystalline phase partially softens. The stationary phase of the polymer material is stretched and oriented under the action of external force, and then rapidly cooled. The stress is frozen by the recrystallization of the reversible phase. When heated again, the reversible phase melts, releasing the tensile stress, and the polymer exhibits macroscopic thermal shrinkage.
[0003] The invention patent with publication number CN103232628B discloses a method for manufacturing a halogen-free flame-retardant heat shrinkable material and a heat shrinkable tube. The halogen-free flame-retardant heat shrinkable material is made of the following raw materials by weight: 100 parts of polyolefin polymer, 10-30 parts of grafting agent, 6-15 parts of composite antioxidant, and 90-140 parts of halogen-free flame retardant. After aging at 135°C for 240 hours, the prepared halogen-free flame retardant material has a breaking strength greater than 8.5MPa and a breaking elongation greater than 200%. It can be used for 60 years at 90°C. After being irradiated with a radiation dose of 2400kGy of gamma rays, the heat shrinkable tube made of the material can still maintain its electrical properties. The material can also withstand the damage of high-temperature and high-pressure water vapor and alkaline solutions. However, the insulation of the halogen-free flame retardant material is poor.
[0004] The invention patent with publication number CN108912506B discloses a semi-rigid heat shrinkable material and a method for manufacturing an integral semi-rigid heat shrinkable umbrella skirt sleeve for high-speed train roof cables. The semi-rigid heat shrinkable material includes polyethylene, ethylene vinyl acetate copolymer, ethylene propylene diene rubber, silicone rubber, filler, lubricant, antioxidant, sensitizing crosslinking agent, light stabilizer, and peroxide crosslinking agent. The sleeve prepared by using the semi-rigid heat shrinkable material overcomes the shortcomings of poor wear resistance and easy breakage, and has good properties of heat shrinkage, mechanical, electrical, flame retardant, corrosion resistance, salt spray resistance, and solvent resistance. However, the insulation of the material is not good. Summary of the invention
[0005] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide a high-strength heat shrinkable tubing material with excellent heat shrinkability, tensile strength, flame retardancy and insulation.
[0006] To achieve the above object, the present invention provides a method for preparing a high-strength heat shrinkable sleeve material, comprising the following steps:
[0007] Step 1, vinyl triethoxysilane, ethylene-vinyl acetate copolymer, dicumyl peroxide, modified copolymer, and hydrotalcite slurry are mixed, extruded and granulated to obtain a mixture A;
[0008] Step 2: Mix polyethylene, antioxidant 1010, benzoyl peroxide, and mixture A prepared in step 1, then extrude and granulate, melt-knead at 160-220° C. to form sheets, and then heat in a water bath for 11-13 hours to obtain a high-strength heat shrinkable tubing material.
[0009] Further preferably, a method for preparing a high-strength heat shrinkable sleeve material comprises the following steps, measured in parts by weight:
[0010] Step 1, 15 to 45 parts of vinyl triethoxysilane, 30 to 75 parts of ethylene-vinyl acetate copolymer, 0.07 to 0.3 parts of dicumyl peroxide, 30 to 60 parts of modified copolymer, and 7.5 to 22.5 parts of hydrotalcite slurry are mixed, extruded and granulated to obtain a mixture A;
[0011] Step 2: 3 to 7 parts of polyethylene, 0.01 to 0.05 parts of antioxidant 1010 and 0.02 to 0.15 parts of benzoyl peroxide, and 55 to 135 parts of the mixture A prepared in step 1 are mixed, followed by extrusion granulation, and then melt-kneading at 160 to 220° C. to produce sheets, and then placed in a water bath at 80 to 100° C. for 11 to 13 hours to obtain a high-strength heat shrinkable tubing material.
[0012] Preferably, in the extrusion granulation, the extrusion temperatures are all independent: five heating zones are set from the feeding section to the die head, and the temperatures are 160-180°C, 160-195°C, 170-200°C, 175-205°C, and 180-210°C respectively.
[0013] Preferably, the modified copolymer is obtained by initially modifying polyisobutylene, then adding acetyltrimethylsilane and octafluoropentyl methacrylate, and finally cross-linking and copolymerizing with octamethylcyclotetrasiloxane.
[0014] Preferably, the modified copolymer is prepared as follows:
[0015] S1. In a water bath at -5 to 0°C, sodium borohydride and tetrahydrofuran are mixed evenly, and then boron trifluoride ether is added dropwise to react for 2 to 4 hours, and then a tetrahydrofuran solution of polyisobutylene is added dropwise, and stirring is continued for 18 to 22 hours, and then the pH is adjusted to 10 to 12 with an aqueous sodium hydroxide solution, and then a hydrogen peroxide solution is added dropwise to react for 7 to 9 hours, and then washed with water, distilled under reduced pressure, and dried in vacuo to obtain primary modified polyisobutylene;
[0016] S2, adding the initially modified polyisobutylene prepared in step S1 to tetrahydrofuran to obtain a tetrahydrofuran solution of initially modified polyisobutylene, and filling with nitrogen for protection; stirring potassium hydride, tetrahydrofuran, and the tetrahydrofuran solution of the initially modified polyisobutylene prepared above at 40-55° C. for 11-13 hours, standing, collecting the supernatant, cooling to room temperature, adding acetyltrimethylsilane and stirring at 40-55° C. for 1-3 hours, then adding octafluoropentyl methacrylate, continuing to stir at 40-55° C. for 1-3 hours, and when the temperature drops to room temperature, adding methanol, stirring for 5-10 minutes, precipitating in n-hexane for 2-4 times, collecting the precipitate, and vacuum drying to obtain an initially modified polymer;
[0017] S3, potassium trimethylsilanol, octamethylcyclotetrasiloxane, and the initially modified polymer prepared in step S2 are mixed, stirred under a nitrogen atmosphere, and heated to 55-80° C., reacted for 3-5 hours, then distilled under reduced pressure, and cooled to room temperature to obtain a modified copolymer.
[0018] Further preferably, the preparation method of the modified copolymer is as follows, in parts by weight:
[0019] S1. Under -5 to 0°C water bath conditions, 20 to 50 parts of sodium borohydride and 30 to 70 parts of tetrahydrofuran are mixed, stirred at 300 to 500 rpm for 10 to 30 minutes, then 10 to 20 parts of boron trifluoride etherate are added dropwise at a rate of 10 to 20 mL / min, reacted for 2 to 4 hours, then 20 to 60 parts of a 60 to 80 wt% tetrahydrofuran solution of polyisobutylene are added dropwise at a rate of 10 to 20 mL / min, and stirred at 300 to 500 rpm for 18 to 22 hours, then the pH is adjusted to 10 to 12 with a 1 to 5 mol / L sodium hydroxide aqueous solution, then 5 to 20 parts of a 65 to 90 wt% hydrogen peroxide aqueous solution are added dropwise at a rate of 5 to 20 mL / min, reacted for 7 to 9 hours, washed with water 2 to 4 times, distilled under reduced pressure at 50 to 80°C for 2 to 4 hours, and vacuum dried for 8 to 12 hours to obtain primary modified polyisobutylene;
[0020] S2, adding 12 to 48 parts of the primary modified polyisobutylene prepared in step S1 to 285 to 1140 parts of tetrahydrofuran to obtain a tetrahydrofuran solution of the primary modified polyisobutylene, and filling with nitrogen for protection; adding 0.2 to 0.8 parts of potassium hydride, 285 to 1140 parts of tetrahydrofuran, and 297 to 1188 parts of the tetrahydrofuran solution of the primary modified polyisobutylene prepared above, stirring at 40 to 55° C. and 300 to 500 rpm for 11 to 13 hours, standing for 2 to 4 hours, collecting the supernatant, and cooling the supernatant to 20 to 30° C. , add 60-90 parts of acetyltrimethylsilane, stir at 40-55°C at 300-500 rpm for 1-3 hours, then add 30-50 parts of octafluoropentyl methacrylate, continue stirring at 40-55°C at 300-500 rpm for 1-3 hours, wait until the temperature drops to 20-30°C, drop 1-3 drops of methanol, stir at 300-500 rpm for 5-10 minutes, precipitate in n-hexane 2-4 times, collect the precipitate, and vacuum dry at 60-85°C for 8-12 hours to obtain a primary modified polymer;
[0021] S3, 0.2-0.5 parts of potassium trimethylsilanol, 50-80 parts of octamethylcyclotetrasiloxane, and 35-93 parts of the primary modified polymer prepared in step S2 are mixed, stirred at 300-500 rpm under a nitrogen atmosphere, and heated to 55-80° C., reacted for 3-5 hours, and then distilled under reduced pressure at 50-70° C. for 2-4 hours, and cooled to 20-30° C. to obtain a modified copolymer.
[0022] Preferably, the preparation method of the hydrotalcite slurry is as follows, in parts by weight:
[0023] 10 to 30 parts of hydrotalcite and 5 to 10 parts of titanate coupling agent are mixed, and ball milled at 400 to 600 revolutions per minute for 1 to 2 hours to obtain hydrotalcite slurry.
[0024] The present invention also provides a method for preparing a high-strength heat shrinkable sleeve, comprising the following steps:
[0025] The high-strength heat shrinkable tube material prepared by the present invention is extruded into a tube by an extruder, and expanded 2 to 5 times at 160 to 220° C. to obtain a high-strength heat shrinkable tube.
[0026] The high-strength heat shrinkable tube prepared by the present invention can be used in the arrangement and protection of cable harnesses in the automotive industry, industrial equipment, and electronic communications, and can also be used in the protection of household wall wires.
[0027] The invention simultaneously grafts acetyltrimethylsilane on polyisobutylene, crosslinks and copolymerizes with octamethylcyclotetrasiloxane under the action of potassium trimethylsilanol to obtain a modified copolymer, and then crosslinks with vinyltriethoxysilane and hydrotalcite slurry to obtain a mixture A, and finally mixes with polyethylene and the like, extrudes, granulates, melts and mixes to obtain sheets, and heats up the sheets to obtain a heat shrinkable tube material. The prepared heat shrinkable tube material has the advantages of good heat shrinkage performance, good flame retardancy, high tensile strength, and good insulation. Acetyltrimethylsilane is grafted onto the modified copolymer, and through the action of trimethylsilanol, octamethylcyclotetrasiloxane is ring-opened and cross-linked with the silyl methyl groups on the grafted acetyltrimethylsilane, thereby generating a large number of silicon-oxygen-silicon bonds and forming a multi-chain network structure, thereby increasing the thermal shrinkage rate and tensile strength of the heat shrinkable tube carbon material. Meanwhile, the ring-opening of octamethylcyclotetrasiloxane and the cross-linking with the silyl methyl groups on the grafted acetyltrimethylsilane can reduce the voids in the heat shrinkable tube material and improve the insulation of the heat shrinkable tube material. The modified copolymer is blended with vinyltriethoxysilane and hydrotalcite slurry, and the vinyltriethoxysilane is cross-linked with the unreacted silyl methyl groups in the modified copolymer. A one-step reaction forms a three-dimensional network structure, in which ethylene-vinyl acetate copolymer and polyethylene are interspersed, thereby increasing the crosslinking degree of the heat shrinkable tube material and the heat shrinkage rate. At the same time, the movement of the molecular chain is hindered, thereby enhancing the tensile strength of the heat shrinkable tube material. The titanate coupling agent improves the compatibility of hydrotalcite with the polymer, and the hydrotalcite slurry is adsorbed in the three-dimensional network structure, thereby increasing the crosslinking points, increasing the crosslinking density of the heat shrinkable tube material, and increasing the heat shrinkage and tensile strength of the heat shrinkable tube material. At the same time, the increase in the crosslinking points reduces the voids in the heat shrinkable tube material and improves the insulation. In addition, the hydrotalcite improves the flame retardancy.
[0028] Due to the adoption of the above technical scheme, compared with the prior art, the present invention has the following advantages: 1) acetyltrimethylsilane is grafted onto the modified copolymer and connected with octamethylcyclotetrasiloxane to form a multi-chain network structure, thereby increasing the thermal shrinkage rate and insulation of the heat shrinkable tube carbon material; 2) the modified copolymer is blended with vinyltriethoxysilane and hydrotalcite slurry, thereby increasing the thermal shrinkage rate, tensile strength, flame retardancy and insulation of the heat shrinkable tube material. DETAILED DESCRIPTION
[0029] Examples and comparative examples Some sources of raw materials:
[0030] Ethylene-vinyl acetate copolymer: Dongguan Jinma Plastic Co., Ltd., brand: 631, item number: AL1157675194.
[0031] Hydrotalcite: fineness: 300-400 mesh. Polyethylene: Dongguan Maoke Plastic Raw Materials Co., Ltd., item number: DGDK-3364.
[0032] Polyisobutylene: Guangzhou Nanjia Chemical Co., Ltd., molecular weight 2400.
[0033] The tetrahydrofuran in the examples was treated as follows before use: dried with potassium hydroxide for three days, added with benzophenone as an indicator, refluxed with sodium wire without oxygen until it turned dark purple, and then evaporated before use.
[0034] The potassium hydride in the example was treated as follows before use: 25 g of potassium hydride was added to 750 g of tetrahydrofuran, stirred and washed at 400 rpm for 8 minutes, the tetrahydrofuran was sucked out after standing, washed 3 times, and the residual tetrahydrofuran was blown out with argon to obtain potassium hydride.
[0035] Titanate coupling agent: Dongguan Dinghai Plastic Chemical Co., Ltd., model NDZ-201.
[0036] Polyethylene: Dongguan Maoke Plastic Raw Materials Co., Ltd., item number: DGDK-3364.
[0037] Example 1
[0038] A method for preparing a high-strength heat shrinkable sleeve material comprises the following steps:
[0039] Step 1, 30g of vinyl triethoxysilane, 50g of ethylene-vinyl acetate copolymer, 0.1g of dicumyl peroxide, 45g of modified copolymer, and 12g of hydrotalcite slurry are mixed, and extruded into granules using a twin-screw extruder, and the twin-screw extruder is provided with five heating zones from the feeding section to the die head, and the temperatures are 170°C, 180°C, 185°C, 190°C, and 195°C, respectively, to obtain a mixture A;
[0040] Step 2: 5 g of polyethylene, 0.02 g of antioxidant 1010, 0.08 g of benzoyl peroxide and 125 g of the mixture A prepared in step 1 are mixed, and then extruded into granules using a twin-screw extruder. Five heating zones are set from the feeding section to the die head of the twin-screw extruder, and the temperatures are 170°C, 180°C, 185°C, 190°C and 195°C respectively. The mixture is melt-kneaded at 200°C to produce a sheet, and then placed in a water bath at 90°C for 12 hours to obtain a high-strength heat shrinkable tubing material.
[0041] The modified copolymer preparation method is as follows:
[0042] S1. In a -1°C water bath, 105 g of sodium borohydride and 165 g of tetrahydrofuran were mixed, stirred at 400 rpm for 20 minutes, and then 45 g of boron trifluoride ether was added dropwise at a rate of 15 mL / min, and the mixture was reacted for 3 hours. Then, 150 g of a 75 wt% polyisobutylene tetrahydrofuran solution was added dropwise at a rate of 15 mL / min, and the mixture was stirred at 400 rpm for 20 hours. Then, the pH was adjusted to 11 with a 2 mol / L sodium hydroxide aqueous solution, and then 45 g of an 80 wt% hydrogen peroxide aqueous solution was added dropwise at a rate of 15 mL / min, and the mixture was reacted for 8 hours. The mixture was washed with water 3 times, and the mixture was distilled at 65°C under reduced pressure for 3 hours, and vacuum dried for 10 hours to obtain primary modified polyisobutylene.
[0043] S2, adding 94.5g of the initially modified polyisobutylene prepared in step S1 to 2250g of tetrahydrofuran to obtain a tetrahydrofuran solution of the initially modified polyisobutylene, and filling with nitrogen for protection; adding 1.8g of potassium hydride, 2250g of tetrahydrofuran, and 2344.5g of the tetrahydrofuran solution of the initially modified polyisobutylene prepared above, stirring at 45°C and 400 rpm for 12 hours, standing for 3 hours, collecting the supernatant, and cooling the supernatant to 25°C, adding 255g of acetyltrimethylsilane, stirring at 45°C and 400 rpm for 2 hours, and then adding 118.5g of octafluoropentyl methacrylate, continuing to stir at 45°C and 400 rpm for 2 hours, and when the temperature drops to 25°C, adding 2 drops of methanol, stirring at 400 rpm for 8 minutes, precipitating in n-hexane 3 times, collecting the precipitate, and vacuum drying at 75°C for 10 hours to obtain an initially modified polymer;
[0044] S3, 1.2g potassium trimethylsilanol, 180g octamethylcyclotetrasiloxane, and 210g of the primary modified polymer prepared in step S2 were mixed, stirred at 400 rpm under a nitrogen atmosphere, and heated to 75°C, reacted for 4 hours, and then distilled under reduced pressure at 65°C for 3 hours, and cooled to 25°C to obtain a modified copolymer.
[0045] The preparation method of the hydrotalcite slurry is as follows: 20 g of hydrotalcite is mixed with 8 g of a titanate coupling agent, and the mixture is ball-milled at 500 rpm for 1.5 hours to obtain the hydrotalcite slurry.
[0046] Comparative Example 1
[0047] A method for preparing a high-strength heat shrinkable sleeve material comprises the following steps:
[0048] Step 1, 50g of ethylene-vinyl acetate copolymer, 0.1g of dicumyl peroxide, 45g of modified copolymer, and 12g of hydrotalcite slurry are mixed, and extruded into granules using a twin-screw extruder, and the twin-screw extruder is provided with five heating zones from the feeding section to the die head, and the temperatures are 170°C, 180°C, 185°C, 190°C, and 195°C, respectively, to obtain a mixture A;
[0049] Step 2: 5 g of polyethylene, 0.02 g of antioxidant 1010, 0.08 g of benzoyl peroxide and 125 g of the mixture A prepared in step 1 are mixed, and then extruded into granules using a twin-screw extruder. Five heating zones are set from the feeding section to the die head of the twin-screw extruder, and the temperatures are 170°C, 180°C, 185°C, 190°C and 195°C respectively. The mixture is melt-kneaded at 200°C to produce a sheet, and then placed in a water bath at 90°C for 12 hours to obtain a high-strength heat shrinkable tubing material.
[0050] The preparation method of the modified copolymer is the same as that of Example 1.
[0051] The preparation method of the hydrotalcite slurry is the same as that of Example 1.
[0052] Comparative Example 2
[0053] The preparation method of a high-strength heat shrinkable tubing material is basically the same as that of Example 1, the only difference being that the preparation method of the modified copolymer is different.
[0054] The modified copolymer preparation method is as follows:
[0055] S1. In a -1°C water bath, 105 g of sodium borohydride and 165 g of tetrahydrofuran were mixed, stirred at 400 rpm for 20 minutes, and then 45 g of boron trifluoride ether was added dropwise at a rate of 15 mL / min, and the mixture was reacted for 3 hours. Then, 150 g of a 75 wt% polyisobutylene tetrahydrofuran solution was added dropwise at a rate of 15 mL / min, and the mixture was stirred at 400 rpm for 20 hours. Then, the pH was adjusted to 11 with a 2 mol / L sodium hydroxide aqueous solution, and then 45 g of an 80 wt% hydrogen peroxide aqueous solution was added dropwise at a rate of 15 mL / min, and the mixture was reacted for 8 hours. The mixture was washed with water 3 times, and the mixture was distilled at 65°C under reduced pressure for 3 hours, and vacuum dried for 10 hours to obtain primary modified polyisobutylene.
[0056] S2, adding 94.5g of the initially modified polyisobutylene prepared in step S1 to 2250g of tetrahydrofuran to obtain a tetrahydrofuran solution of the initially modified polyisobutylene, and filling with nitrogen for protection; adding 1.8g of potassium hydride, 2250g of tetrahydrofuran, and 2344.5g of the tetrahydrofuran solution of the initially modified polyisobutylene prepared above, stirring at 45°C and 400 rpm for 12 hours, standing for 3 hours, collecting the supernatant, and cooling the supernatant to 25°C, adding 118.5g of octafluoropentyl methacrylate, stirring at 45°C and 400 rpm for 2 hours, and when the temperature drops to 25°C, adding 2 drops of methanol, stirring at 400 rpm for 8 minutes, precipitating in n-hexane 3 times, collecting the precipitate, and vacuum drying at 75°C for 10 hours to obtain an initially modified polymer;
[0057] S3, 1.2g potassium trimethylsilanol, 180g octamethylcyclotetrasiloxane, and 210g of the primary modified polymer prepared in step S2 were mixed, stirred at 400 rpm under a nitrogen atmosphere, and heated to 75°C, reacted for 4 hours, and then distilled under reduced pressure at 65°C for 3 hours, and cooled to 25°C to obtain a modified copolymer.
[0058] The preparation method of the hydrotalcite slurry is the same as that of Example 1.
[0059] Comparative Example 3
[0060] A method for preparing a high-strength heat shrinkable sleeve material comprises the following steps:
[0061] Step 1, 30g of vinyl triethoxysilane, 50g of ethylene-vinyl acetate copolymer, 0.1g of dicumyl peroxide, and 12g of hydrotalcite slurry are mixed, and extruded into granules using a twin-screw extruder, wherein five heating zones are set from the feeding section to the die head of the twin-screw extruder, and the temperatures are 170°C, 180°C, 185°C, 190°C, and 195°C, respectively, to obtain a mixture A;
[0062] Step 2: 5 g of polyethylene, 0.02 g of antioxidant 1010, 0.08 g of benzoyl peroxide and 125 g of the mixture A prepared in step 1 are mixed, and then extruded into granules using a twin-screw extruder. Five heating zones are set from the feeding section to the die head of the twin-screw extruder, and the temperatures are 170°C, 180°C, 185°C, 190°C and 195°C respectively. The mixture is melt-kneaded at 200°C to produce a sheet, and then placed in a water bath at 90°C for 12 hours to obtain a high-strength heat shrinkable tubing material.
[0063] The preparation method of the hydrotalcite slurry is the same as that of Example 1.
[0064] Comparative Example 4
[0065] A method for preparing a high-strength heat shrinkable sleeve material comprises the following steps:
[0066] Step 1, 30g of vinyl triethoxysilane, 50g of ethylene-vinyl acetate copolymer, 0.1g of dicumyl peroxide, and 45g of modified copolymer are mixed, and extruded into granules using a twin-screw extruder, and the twin-screw extruder is provided with five heating zones from the feeding section to the die head, and the temperatures are 170°C, 180°C, 185°C, 190°C, and 195°C, respectively, to obtain a mixture A;
[0067] Step 2: 5 g of polyethylene, 0.02 g of antioxidant 1010, 0.08 g of benzoyl peroxide and 125 g of the mixture A prepared in step 1 are mixed, and then extruded into granules using a twin-screw extruder. Five heating zones are set from the feeding section to the die head of the twin-screw extruder, and the temperatures are 170°C, 180°C, 185°C, 190°C and 195°C respectively. The mixture is melt-kneaded at 200°C to produce a sheet, and then placed in a water bath at 90°C for 12 hours to obtain a high-strength heat shrinkable tubing material.
[0068] The preparation method of the modified copolymer is the same as that of Example 1.
[0069] Test Example 1
[0070] Heat shrinkage performance test:
[0071] The heat shrink performance test of the high-strength heat shrinkable tubing material prepared by the present invention was carried out with reference to the national standard of the People's Republic of China GB / T34848-2017 "Test Method for Shrinkage Performance of Heat Shrinkable Films", and the sample was prepared along the transverse direction of the sample. The sample width was 5 mm and the sample length was 120 mm. Before the test, the sample was placed in a standard environment with a temperature of 23°C and a relative humidity of 50% for 4 hours. Three parallels were made for each sample, and the average value was taken. The results are shown in Table 1:
[0072] Test Example 2
[0073] Tensile strength test:
[0074] The tensile strength test of the heat shrinkable tubing material prepared by the present invention was carried out with reference to the national standards of the People's Republic of China GB / T1040.1-2006 "Determination of tensile properties of plastics Part 1: General principles" and GB / T1040.2-2006 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics". The test selected a dumbbell shape of type 1A, the test speed was 50 mm / min, three parallels were made for each sample, and the average value was taken. The results are shown in Table 1.
[0075] Test Example 3
[0076] Flame retardancy test:
[0077] The flame retardancy test of the heat shrinkable material prepared by the present invention was carried out with reference to the national standard of the People's Republic of China GB / T2406.2-2009 "Determination of Combustion Behavior of Plastics by Oxygen Index Method Part 2: Room Temperature Test". The combustion tube is 500 mm high and 80 mm in inner diameter. The exhaust gas flow rate of the combustion tube is 100 mm / s. Clean air containing 20.9 vt% oxygen is used as the gas source. The sample is cut into a size of 100 mm in length, 10 mm in width and 4 mm in thickness. The sample is ignited by the top surface ignition method. 15 parallels are made for each sample, and the average value is taken. The results are shown in Table 1.
[0078] Test Example 4
[0079] Insulation test:
[0080] The insulation properties of the heat shrinkable tubing material prepared by the present invention were tested with reference to the National Standard of the People's Republic of China GB / T31838.2-2019 "Dielectric and Resistive Properties of Solid Insulating Materials Part 2: Resistance Characteristics (DC Method) Volume Resistance and Volume Resistivity". The volume resistivity was used as the test index. The sample was placed in an environment with a temperature of 23°C and a relative humidity of 50% for 5 days before the test. Three parallel samples were made for each sample, and the average value was taken. The results are shown in Table 1.
[0081] Table 1 Test results
[0082]
[0083] (Note: The larger the oxygen index, the better the flame retardancy; the larger the volume resistivity, the better the insulation.)
[0084] By comparing Example 1 with Comparative Examples 1 to 4, it can be found that the heat shrinkage, tensile strength, flame retardancy and insulation of Example 1 are all better than those of Comparative Examples 1 to 4. This may be because the octamethylcyclotetrasiloxane in Example 1 is ring-opened and connected to the silyl methyl group on the grafted acetyltrimethylsilane, thereby increasing the heat shrinkage, tensile strength and insulation of the heat shrinkable tube carbon material; the modified copolymer is blended with vinyltriethoxysilane and hydrotalcite slurry, and vinyltriethoxysilane and the modified copolymer form a three-dimensional network structure, in which ethylene-vinyl acetate copolymer and polyethylene are interspersed, thereby increasing the heat shrinkage and tensile strength; the titanate coupling agent improves the compatibility of hydrotalcite with the polymer, and the hydrotalcite slurry is adsorbed in the three-dimensional network structure, thereby increasing the heat shrinkage, tensile strength, insulation and flame retardancy of the heat shrinkable tube material.
Claims
1. A high-strength heat shrinkable tubing material, characterized in that: Prepared by the following method: Step 1, vinyl triethoxysilane, ethylene-vinyl acetate copolymer, dicumyl peroxide, modified copolymer, and hydrotalcite slurry are mixed, extruded and granulated to obtain a mixture A; Step 2, polyethylene, antioxidant 1010, benzoyl peroxide, and the mixture A prepared in step 1 are mixed, followed by extrusion granulation, and then melt-kneading at 160-220° C. to form a sheet, and then heated in a water bath for 11-13 hours to obtain a high-strength heat shrinkable tubing material; The modified copolymer is obtained by first modifying polyisobutylene, then adding acetyltrimethylsilane and octafluoropentyl methacrylate, and finally cross-linking and copolymerizing with octamethylcyclotetrasiloxane; The modified copolymer preparation method is as follows: S1. In a water bath at -5 to 0°C, mix sodium borohydride and tetrahydrofuran evenly, then drop boron trifluoride etherate, react for 2 to 4 hours, then drop a tetrahydrofuran solution of polyisobutylene, continue stirring for 18 to 22 hours, then adjust the pH to 10 to 12 with a sodium hydroxide aqueous solution, then drop a hydrogen peroxide solution, react for 7 to 9 hours, wash with water, distill under reduced pressure, and dry in vacuum to obtain primary modified polyisobutylene; S2, adding the initially modified polyisobutylene to tetrahydrofuran to obtain a tetrahydrofuran solution of the initially modified polyisobutylene, and filling with nitrogen for protection; stirring potassium hydride, tetrahydrofuran, and the tetrahydrofuran solution of the initially modified polyisobutylene at 40-55° C. for 11-13 hours, standing, collecting the supernatant, cooling to room temperature, adding acetyltrimethylsilane, stirring at 40-55° C. for 1-3 hours, then adding octafluoropentyl methacrylate, continuing to stir at 40-55° C. for 1-3 hours, and when the temperature drops to room temperature, adding methanol, stirring for 5-10 minutes, precipitating in n-hexane for 2-4 times, collecting the precipitate, and vacuum drying to obtain an initially modified polymer; S3. Mix potassium trimethylsilanol, octamethylcyclotetrasiloxane and the primary modified polymer, stir under a nitrogen atmosphere, and heat to 55-80° C., react for 3-5 hours, then reduce the pressure, distill, and cool to room temperature to obtain a modified copolymer.
2. The high-strength heat shrinkable tubing material according to claim 1, characterized in that: In step S1, the mass ratio of sodium borohydride, tetrahydrofuran, boron trifluoride etherate, tetrahydrofuran solution of polyisobutylene, and hydrogen peroxide solution is 20-50:30-70:10-20:20-60:5-20, the concentration of the tetrahydrofuran solution of polyisobutylene is 60-80wt%, and the concentration of the hydrogen peroxide solution is 65-90vt; in step S2, the tetrahydrofuran solution of primary modified polyisobutylene, potassium hydride, tetrahydrofuran, acetyltrimethylsilane The mass ratio of alkane and octafluoropentyl methacrylate is 297~1188:0.2~0.8:285~1140:60~90:30~50, the mass ratio of the primary modified polyisobutylene to tetrahydrofuran in the tetrahydrofuran solution of the primary modified polyisobutylene is 12~48:285~1140; the mass ratio of potassium trimethylsilanol, octamethylcyclotetrasiloxane and the primary modified polymer in step S3 is 0.2~0.5:50~80:35~93.
3. The high-strength heat shrinkable tubing material according to claim 1, characterized in that: The preparation method of the hydrotalcite slurry is as follows, in parts by weight: 10 to 30 parts of hydrotalcite are mixed with 5 to 10 parts of titanate coupling agent, and ball milled at 400 to 600 rpm for 1 to 2 hours to obtain the hydrotalcite slurry.
4. The high-strength heat shrinkable tubing material according to claim 1, characterized in that: In the step 1, the mass ratio of vinyl triethoxysilane, ethylene-vinyl acetate copolymer, dicumyl peroxide, modified copolymer and hydrotalcite slurry is 15-45:30-75:0.07-0.3:30-60:7.5-22.5; In the step 2, the mass ratio of polyethylene, antioxidant 1010, benzoyl peroxide and mixture A is 3-7:0.01-0.05:0.02-0.15:55-135.
5. The high-strength heat shrinkable tubing material according to claim 1, characterized in that: The extrusion granulation has various independent extrusion temperatures: five heating zones are set from the feeding section to the die head, and the temperatures are 160-180°C, 160-195°C, 170-200°C, 175-205°C, and 180-210°C respectively.
6. The high-strength heat shrinkable tubing material according to claim 1, characterized in that: The steps include: Step 1, 30g of vinyl triethoxysilane, 50g of ethylene-vinyl acetate copolymer, 0.1g of dicumyl peroxide, 45g of modified copolymer, and 12g of hydrotalcite slurry are mixed, and extruded into granules using a twin-screw extruder, and the twin-screw extruder is provided with five heating zones from the feeding section to the die head, and the temperatures are 170°C, 180°C, 185°C, 190°C, and 195°C, respectively, to obtain a mixture A; Step 2, 5g polyethylene, 0.02g antioxidant 1010 and 0.08g benzoyl peroxide, 125g mixture A prepared in step 1 are mixed, and then extruded into granules using a twin-screw extruder, and the twin-screw extruder is provided with five heating zones from the feeding section to the die head, and the temperatures are 170°C, 180°C, 185°C, 190°C, and 195°C, respectively, and then melt-mixed at 200°C to form a sheet, and then placed in a water bath at 90°C for 12 hours to obtain a high-strength heat shrinkable sleeve material; The modified copolymer preparation method is as follows: S1. In a -1°C water bath, 105 g of sodium borohydride and 165 g of tetrahydrofuran were mixed, stirred at 400 rpm for 20 minutes, and then 45 g of boron trifluoride ether was added dropwise at a rate of 15 mL / min, and the mixture was reacted for 3 hours. Then, 150 g of a 75 wt% polyisobutylene tetrahydrofuran solution was added dropwise at a rate of 15 mL / min, and the mixture was stirred at 400 rpm for 20 hours. Then, the pH was adjusted to 11 with a 2 mol / L sodium hydroxide aqueous solution, and then 45 g of an 80 wt% hydrogen peroxide aqueous solution was added dropwise at a rate of 15 mL / min, and the mixture was reacted for 8 hours. The mixture was washed with water 3 times, and the mixture was distilled at 65°C under reduced pressure for 3 hours, and vacuum dried for 10 hours to obtain the primary modified polyisobutylene. S2, adding 94.5g of the initially modified polyisobutylene prepared in step S1 to 2250g of tetrahydrofuran to obtain a tetrahydrofuran solution of the initially modified polyisobutylene, and filling with nitrogen for protection; adding 1.8g of potassium hydride, 2250g of tetrahydrofuran, and 2344.5g of the tetrahydrofuran solution of the initially modified polyisobutylene prepared above, stirring at 45°C and 400 rpm for 12 hours, standing for 3 hours, collecting the supernatant, and cooling the supernatant to 25°C, adding 255g of acetyltrimethylsilane, stirring at 45°C and 400 rpm for 2 hours, and then adding 118.5g of octafluoropentyl methacrylate, continuing to stir at 45°C and 400 rpm for 2 hours, and when the temperature drops to 25°C, adding 2 drops of methanol, stirring at 400 rpm for 8 minutes, precipitating in n-hexane 3 times, collecting the precipitate, and vacuum drying at 75°C for 10 hours to obtain an initially modified polymer; S3, 1.2 g of potassium trimethylsilanol, 180 g of octamethylcyclotetrasiloxane, and 210 g of the primary modified polymer prepared in step S2 were mixed, stirred at 400 rpm under a nitrogen atmosphere, and heated to 75° C., reacted for 4 hours, and then distilled under reduced pressure at 65° C. for 3 hours, and cooled to 25° C. to obtain a modified copolymer; The preparation method of the hydrotalcite slurry is as follows: 20 g of hydrotalcite is mixed with 8 g of a titanate coupling agent, and the mixture is ball-milled at 500 rpm for 1.5 hours to obtain the hydrotalcite slurry.
7. A high-strength heat shrinkable tube, characterized in that: The high-strength heat shrinkable tube material according to any one of claims 1 to 5 is extruded into a tube by an extruder, and expanded by 2 to 5 times at 160 to 220° C. to obtain a high-strength heat shrinkable tube.
8. The high-strength heat shrinkable tube described in claim 7 can be used in the arrangement and protection of cable harnesses in the automotive industry, industrial equipment, and electronic communications, and can also be used in the protection of household wall wires.
9. A modified copolymer, characterized in that: The following preparation method is used to prepare: S1. In a water bath at -5 to 0°C, mix sodium borohydride and tetrahydrofuran evenly, then drop boron trifluoride etherate, react for 2 to 4 hours, then drop a tetrahydrofuran solution of polyisobutylene, continue stirring for 18 to 22 hours, then adjust the pH to 10 to 12 with a sodium hydroxide aqueous solution, then drop a hydrogen peroxide solution, react for 7 to 9 hours, wash with water, distill under reduced pressure, and dry in vacuum to obtain primary modified polyisobutylene; S2, adding the initially modified polyisobutylene to tetrahydrofuran to obtain a tetrahydrofuran solution of the initially modified polyisobutylene, and filling with nitrogen for protection; stirring potassium hydride, tetrahydrofuran, and the tetrahydrofuran solution of the initially modified polyisobutylene prepared above at 40-55° C. for 11-13 hours, standing, collecting the supernatant, cooling to room temperature, adding acetyltrimethylsilane and stirring at 40-55° C. for 1-3 hours, then adding octafluoropentyl methacrylate, continuing to stir at 40-55° C. for 1-3 hours, and when the temperature drops to room temperature, adding methanol, stirring for 5-10 minutes, precipitating in n-hexane for 2-4 times, collecting the precipitate, and vacuum drying to obtain an initially modified polymer; S3, potassium trimethylsilanol, octamethylcyclotetrasiloxane and the primary modified polymer are mixed, stirred under a nitrogen atmosphere, and heated to 55-80° C., reacted for 3-5 hours, and then decompressed, distilled, and cooled to room temperature to obtain a modified copolymer; In step S1, the mass ratio of sodium borohydride, tetrahydrofuran, boron trifluoride etherate, tetrahydrofuran solution of polyisobutylene, and hydrogen peroxide solution is 20-50:30-70:10-20:20-60:5-20, the concentration of the tetrahydrofuran solution of polyisobutylene is 60-80wt%, and the concentration of the hydrogen peroxide solution is 65-90vt; in step S2, the tetrahydrofuran solution of primary modified polyisobutylene, potassium hydride, tetrahydrofuran, acetyltrimethylsilane The mass ratio of alkane and octafluoropentyl methacrylate is 297~1188:0.2~0.8:285~1140:60~90:30~50, the mass ratio of the primary modified polyisobutylene to tetrahydrofuran in the primary modified polyisobutylene tetrahydrofuran solution is 12~48:285~1140; the mass ratio of potassium trimethylsilanol, octamethylcyclotetrasiloxane and primary modified polymer in step S3 is 0.2~0.5:50~80:35~93.