Biomass carbon ball, preparation method thereof, antistatic composite material and preparation method thereof

The preparation of biomass carbon spheres through hydrothermal reaction and the ultrasonic reaction of polyorganic acids is solved, and the compatibility and cost problems of PBAT materials in electromagnetic shielding, conductivity and anti-static are achieved, and high-efficiency and low-cost conductive properties and mechanics are achieved. Improved performance and suitable for antistatic materials.

CN116041989BActive Publication Date: 2024-11-22JUNENG NEW MATERIAL TECH (JINGMEN) CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202310031942.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-10
Publication Date
2024-11-22
Estimated Expiration
2043-01-10

AI Technical Summary

Technical Problem

In the prior art, the modification of PBAT materials in electromagnetic shielding, conductivity, antistatic and other aspects has problems such as high cost, complex production process and poor compatibility. The commonly used carbon materials are expensive and the production process is complex, so they cannot effectively reduce the composite. The cost of the material.

Method used

Biomass carbon spheres are prepared through hydrothermal reactions, and the hydrolysis is accelerated by persulfate, forming a variety of organic acids, thereby increasing the number of carbon sphere cores and carbonization degree, combining with ultrasonic reactions of multiple organic acids, forming nanocarbon spheres, improving the PBAT Compatibility and antistatic composite materials are prepared by melt blending.

Benefits of technology

It achieves good compatibility between biomass carbon spheres and PBAT, reduces production costs, improves conductive and mechanical properties, simplifies the process flow, and is safe and environmentally friendly, suitable for the field of antistatic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116041989B_ABST
    Figure CN116041989B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of polymer materials, and in particular, relates to a biomass carbon ball, a preparation method thereof, an antistatic composite material and a preparation method thereof. The biomass carbon ball provided by the present invention is prepared by hydrothermal reaction of biomass powder and persulfate, followed by washing, drying and oxygen-free calcination, and then ultrasonic reaction with polybasic organic acid in an organic solvent, followed by washing, drying and grinding. The biomass carbon ball provided by the present invention has good compatibility with PBAT, and the biomass raw materials used to prepare the biomass carbon ball are not limited to pure sugar substances. The raw material sources are wide, the preparation process is simple, safe and environmentally friendly, low cost, and high yield; the antistatic composite material provided by the present invention uses PBAT as a base material, and is added with the biomass carbon ball provided by the present invention, and has very excellent electrical conductivity and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a biomass carbon ball, a preparation method thereof, an antistatic composite material and a preparation method thereof. Background Art

[0002] Polybutylene adipate-terephthalate (PBAT) is a new type of biodegradable material commonly used at present, which is mainly used in agricultural mulch and food packaging. However, PBAT has problems such as poor crystallinity, low melt strength and high price. Therefore, it is necessary to modify PBAT, mainly by blending modification and chain extension modification, in order to reduce costs and improve its comprehensive performance. In the modification of electromagnetic shielding, conductivity, antistatic and other aspects, the commonly used materials in the literature reported at present are graphene, carbon nanotubes, etc., but these carbon materials are not only expensive, but also complicated in production process, and have poor compatibility with PBAT, and also need surface activation treatment to introduce hydrophilic groups.

[0003] In contrast, biomass carbon has the advantages of a wide range of raw material sources, low cost and renewability, which can effectively reduce the cost of composite materials. In particular, biomass spherical carbon materials have attracted great attention from the scientific community for their high specific surface area, good conductivity, adjustable porosity, surface functionalization, ordered porous structure, controllable particle size and morphology distribution, excellent active sites, mechanical and thermal stability. The most important point is that the biomass carbon spheres prepared by the hydrothermal carbonization method will selectively aggregate hydrophilic functional groups such as hydroxyl and carboxyl on the surface of the carbon spheres during the nucleation and growth process, which will undoubtedly greatly increase the compatibility with PBAT, and the prepared carbon sphere material does not require additional modification.

[0004] However, the biomass carbon sources currently used to synthesize carbon balls are mostly pure sugar substances. These materials have relatively simple structures and are themselves industrial products. The use of them to prepare functional carbon ball materials has problems such as high production costs, complex raw material source processes, and insignificant economic benefits. In addition, the above processes require high temperatures or strong acid and alkali reagents, which cannot achieve green preparation and cannot be extended to plant-based biomass with complex structures and protection such as complete cell wall structures. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a biomass carbon ball, a preparation method thereof, an antistatic composite material and a preparation method thereof. The biomass carbon ball provided by the present invention has good compatibility with PBAT, and the biomass raw materials used to prepare the biomass carbon ball are not limited to pure sugar substances. The raw material source is wide, the preparation process is simple, safe and environmentally friendly, low cost, and high yield; the antistatic composite material provided by the present invention uses PBAT as a base material and is added with the biomass carbon ball provided by the present invention, and has very excellent conductive properties and mechanical properties.

[0006] The invention provides a biomass carbon ball, which is prepared by hydrothermal reaction of biomass powder and persulfate, followed by washing, drying and oxygen-free calcination, ultrasonic reaction with polybasic organic acid in an organic solvent, and subsequent washing, drying and grinding.

[0007] Preferably, the biomass powder is one or more of sunflower seed shell powder, sunflower stem powder, rice straw powder, rice husk powder, corn straw powder, sisal powder, jute powder, peanut shell powder, fir bark powder, pine cone powder, bamboo shoot shell powder, coconut shell powder, nut shell powder and soybean pod powder.

[0008] Preferably, the persulfate is one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

[0009] Preferably, the polybasic organic acid is one or more of citric acid, tartaric acid, malic acid, salicylic acid, alginic acid and quinic acid.

[0010] Preferably, based on 100 parts by weight of the biomass powder, the amount of the persulfate is 200-400 parts by weight, and the amount of the polybasic organic acid is 20-30 parts by weight.

[0011] The present invention provides a method for preparing biomass carbon balls as described in the above technical solution, comprising the following steps:

[0012] a) subjecting biomass powder and persulfate to a hydrothermal reaction; after the reaction is completed, washing and drying the reaction product to obtain a dried material;

[0013] b) calcining the dried material in the absence of oxygen to obtain a pyrolysis material;

[0014] c) mixing the pyrolysis material and polybasic organic acid in an organic solvent and subjecting the mixture to ultrasonic reaction; after the reaction is completed, washing, drying and grinding the reaction product to obtain biomass carbon balls.

[0015] Preferably, in step a), the temperature of the hydrothermal reaction is 220-240° C.; the time of the hydrothermal reaction is 12-24 hours;

[0016] In step b), the temperature of the oxygen-free calcination is 500-600° C.; the time of the oxygen-free calcination is 60-100 min;

[0017] In step c), the ultrasonic frequency of the ultrasonic reaction is 40-60 KHz; the temperature of the ultrasonic reaction is 60-80° C.; and the time of the ultrasonic reaction is 20-40 min.

[0018] The present invention provides an antistatic composite material, which is prepared by melt blending raw materials, wherein the raw materials include biomass carbon balls, polybutylene adipate-terephthalate, a dispersant and a chain extender;

[0019] The biomass carbon balls are the biomass carbon balls described in the above technical solution or the biomass carbon balls prepared by the preparation method described in the above technical solution.

[0020] The present invention provides a method for preparing the antistatic composite material described in the above technical solution, comprising the following steps:

[0021] The biomass carbon balls, polybutylene adipate-terephthalate, a dispersant and a chain extender are melt-blended to obtain an antistatic composite material.

[0022] Preferably, the melt blending is carried out in a screw extruder; the extrusion speed of the screw extruder is 100-200 rpm; the temperature of the blending section of the screw extruder is 160-180°C; the temperature of the extrusion section of the screw extruder is 150-170°C.

[0023] Compared with the prior art, the present invention provides a biomass carbon ball, a preparation method thereof, an antistatic composite material and a preparation method thereof. The biomass carbon ball provided by the present invention is prepared by hydrothermal reaction of biomass powder and persulfate, followed by washing, drying and oxygen-free calcination, and then ultrasonic reaction with polybasic organic acid in an organic solvent, followed by washing, drying and grinding. The present invention increases the compatibility with PBAT by means of hydrophilic functional groups such as hydroxyl and carboxyl groups gathered on the surface of carbon balls during the formation of hydrothermal carbon balls, and the prepared carbon ball material does not require additional modification treatment; persulfate is used to accelerate the hydrolysis of biomass, decompose a variety of organic acids, thereby forming more aromatic compounds, greatly increase the number of carbon ball cores, prepare nano carbon balls with smaller particle size, accelerate the hydrothermal reaction process, improve the yield and promote the degree of carbonization; polybasic organic acids are used to remove tar in the pores of carbon materials under the assistance of ultrasound, and polybasic organic acids are used as compatibilizers to further improve the compatibility of carbon balls with PBAT. The biomass carbon balls provided by the present invention have good compatibility with PBAT, and the biomass raw materials used to prepare the biomass carbon balls are not limited to pure sugar substances. The raw material sources are wide, the preparation process is simple, safe and environmentally friendly, low cost, high yield, and have good economic and environmental benefits. The antistatic composite material provided by the present invention is made by melt blending of raw materials, and the raw materials include biomass carbon balls, polybutylene adipate-terephthalate, a dispersant and a chain extender; the biomass carbon balls are the biomass carbon balls described in the above technical scheme or the biomass carbon balls prepared by the preparation method described in the above technical scheme. The antistatic composite material provided by the present invention is made by reactive melt blending of the biomass carbon balls provided by the present invention and PBAT, and has very excellent electrical conductivity and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0025] Figure 1 is a scanning electron microscope image of the biomass carbon sphere provided in Example 1 of the present invention;

[0026] Figure 2 This is a scanning electron microscope image of the biomass carbon material provided in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The invention provides a biomass carbon ball, which is prepared by hydrothermal reaction of biomass powder and persulfate, followed by washing, drying and oxygen-free calcination, ultrasonic reaction with polybasic organic acid in an organic solvent, and subsequent washing, drying and grinding.

[0029] In the biomass carbon balls provided by the present invention, the biomass powder is preferably one or more of sunflower seed shell powder, sunflower stem powder, rice straw powder, rice husk powder, corn straw powder, sisal powder, jute powder, peanut shell powder, fir bark powder, pine cone powder, bamboo shoot shell powder, coconut shell powder, nut shell powder and soybean pod powder. In one embodiment provided by the present invention, the biomass powder is rice husk powder and corn straw powder, and the mass ratio of the rice husk powder to the corn straw powder is preferably 1: (0.5-2), more preferably 1: 1; in one embodiment provided by the present invention, the biomass powder is sisal powder and jute powder, and the mass ratio of the sisal powder to the jute powder is preferably 1: (0.5-2), more preferably 1: 1; in one embodiment provided by the present invention, the biomass powder is sunflower seed shell powder, peanut shell powder and coconut shell powder, and the mass ratio of the sunflower seed shell powder, peanut shell powder and coconut shell powder is preferably 3: (2-6): (2-6), more preferably 3: 3: 4.

[0030] In the biomass carbon balls provided by the present invention, the mesh number of the biomass powder is 400-600 mesh, specifically 400 mesh, 410 mesh, 420 mesh, 430 mesh, 440 mesh, 450 mesh, 460 mesh, 470 mesh, 480 mesh, 490 mesh, 500 mesh, 510 mesh, 520 mesh, 530 mesh, 540 mesh, 550 mesh, 560 mesh, 570 mesh, 580 mesh, 590 mesh or 600 mesh.

[0031] In the biomass carbon spheres provided by the present invention, the persulfate is preferably one or more of ammonium persulfate, potassium persulfate and sodium persulfate. In one embodiment provided by the present invention, the persulfate is ammonium persulfate and potassium persulfate, and the mass ratio of the ammonium persulfate to the potassium persulfate is preferably 2: (1 to 3), more preferably 2: 1.5. In one embodiment provided by the present invention, the persulfate is potassium persulfate and sodium persulfate, and the mass ratio of the potassium persulfate to the sodium persulfate is preferably 1: (0.5 to 2), more preferably 1: 1.

[0032] In the biomass carbon balls provided by the present invention, based on 100 parts by weight of the biomass powder, the amount of the persulfate is preferably 200-400 parts by weight, specifically 200 parts by weight, 210 parts by weight, 220 parts by weight, 230 parts by weight, 240 parts by weight, 250 parts by weight, 260 parts by weight, 270 parts by weight, 280 parts by weight, 290 parts by weight, 300 parts by weight, 310 parts by weight, 320 parts by weight, 330 parts by weight, 340 parts by weight, 350 parts by weight, 360 parts by weight, 370 parts by weight, 380 parts by weight, 390 parts by weight or 400 parts by weight.

[0033] In the biomass carbon balls provided by the present invention, the hydrothermal reaction is carried out in a closed reactor. Based on 100 parts by weight of the biomass powder, the amount of water used in the hydrothermal reaction is preferably 1000 to 3000 parts by weight, specifically 1000 parts by weight, 1200 parts by weight, 1500 parts by weight, 1700 parts by weight, 2000 parts by weight, 2300 parts by weight, 2500 parts by weight, 2700 parts by weight or 3000 parts by weight.

[0034] In the biomass carbon balls provided by the present invention, the organic solvent is preferably ethanol, more preferably anhydrous ethanol; based on 100 parts by weight of the biomass powder, the amount of the organic solvent is preferably 300 to 600 parts by weight, specifically 300 parts by weight, 350 parts by weight, 400 parts by weight, 450 parts by weight, 500 parts by weight, 550 parts by weight or 600 parts by weight.

[0035] In the biomass carbon balls provided by the present invention, the polybasic organic acid is preferably one or more of citric acid, tartaric acid, malic acid, salicylic acid, alginic acid and quinic acid. In one embodiment provided by the present invention, the polybasic organic acid is malic acid and salicylic acid, and the mass ratio of malic acid to salicylic acid is preferably 12: (7-20), more preferably 12: 13. In one embodiment provided by the present invention, the polybasic organic acid is citric acid, salicylic acid and alginic acid, and the mass ratio of citric acid, salicylic acid and alginic acid is preferably 1: (0.5-2): (0.5-2), more preferably 1: 1: 1.

[0036] In the biomass carbon balls provided by the present invention, based on 100 parts by weight of the biomass powder, the amount of the polybasic organic acid is preferably 20 to 30 parts by weight, specifically 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight or 30 parts by weight.

[0037] In the biomass carbon balls provided by the present invention, the mesh number of the biomass carbon balls is preferably 800-1000 mesh, specifically 800 mesh, 810 mesh, 820 mesh, 830 mesh, 840 mesh, 850 mesh, 860 mesh, 870 mesh, 880 mesh, 890 mesh, 900 mesh, 910 mesh, 920 mesh, 930 mesh, 940 mesh, 950 mesh, 960 mesh, 970 mesh, 980 mesh, 990 mesh or 1000 mesh.

[0038] The present invention also provides a method for preparing the biomass carbon balls described in the above technical solution, comprising the following steps:

[0039] a) subjecting biomass powder and persulfate to a hydrothermal reaction; after the reaction is completed, washing and drying the reaction product to obtain a dried material;

[0040] b) calcining the dried material in the absence of oxygen to obtain a pyrolysis material;

[0041] c) mixing the pyrolysis material and polybasic organic acid in an organic solvent and subjecting the mixture to ultrasonic reaction; after the reaction is completed, washing, drying and grinding the reaction product to obtain biomass carbon balls.

[0042] In the preparation method provided by the present invention, in step a), the specific types and usage ratios of the biomass powder and persulfate have been introduced above and will not be repeated here.

[0043] In the preparation method provided by the present invention, in step a), the hydrothermal reaction is carried out in a closed reactor; the temperature of the hydrothermal reaction is preferably 220-240°C, specifically 220°C, 221°C, 222°C, 223°C, 224°C, 225°C, 226°C, 227°C, 228°C, 229°C, 230°C, 231°C, 232°C, 233°C, 234°C, 235°C, 236°C, 237°C, 238°C, 239°C or 240°C; the time of the hydrothermal reaction is preferably 12-24h, specifically 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h.

[0044] In the preparation method provided by the present invention, in step a), the reaction product is a solid material obtained by filtration after the reaction is completed; the washing is preferably water washing; the drying method is preferably oven drying, and the drying temperature is preferably 60-80°C, specifically 60°C, 65°C, 70°C, 75°C or 80°C.

[0045] In the preparation method provided by the present invention, in step b), the oxygen-free calcination is preferably carried out in an inert gas atmosphere, and the inert gas is preferably argon; the temperature of the oxygen-free calcination is preferably 500-600°C, specifically 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C; the time of the oxygen-free calcination is preferably 60-100 min, specifically 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, 90 min, 95 min or 100 min. In the present invention, the heating rate before reaching the temperature is preferably 5 to 10°C / min, specifically 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min; the cooling rate after completing the oxygen-free calcination is preferably 5 to 10°C / min, specifically 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min.

[0046] In the preparation method provided by the present invention, in step c), the specific types and usage ratios of the organic solvent and the polybasic organic acid have been introduced above and will not be repeated here.

[0047] In the preparation method provided by the present invention, in step c), the ultrasonic frequency of the ultrasonic reaction is preferably 40-60KHz, specifically 40KHz, 41KHz, 42KHz, 43KHz, 44KHz, 45KHz, 46KHz, 47KHz, 48KHz, 49KHz, 50KHz, 51KHz, 52KHz, 53KHz, 54KHz, 55KHz, 56KHz, 57KHz, 58KHz, 59KHz or 60KHz; the temperature of the ultrasonic reaction is preferably 60-80°C, specifically 60°C, 61°C, 62°C, 63°C, 64°C, the ultrasonic reaction time is preferably 20 to 40 min, specifically 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min, 30 min, 31 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 39 min or 40 min.

[0048] In the preparation method provided by the present invention, in step c), the reaction product is a solid material obtained by filtration after the reaction is completed; the washing is preferably water washing; the drying method is preferably oven drying, and the drying temperature is preferably 60-80°C, specifically 60°C, 65°C, 70°C, 75°C or 80°C; the grinding method is preferably ball milling.

[0049] The present invention also provides an antistatic composite material, which is made by melt blending of raw materials, wherein the raw materials include biomass carbon balls, polybutylene adipate-terephthalate, a dispersant and a chain extender; the biomass carbon balls are the biomass carbon balls described in the above technical scheme or the biomass carbon balls prepared by the preparation method described in the above technical scheme.

[0050] In the antistatic composite material provided by the present invention, the molar ratio of the aliphatic polyester (BA) repeating unit to the aromatic polyester (BT) repeating unit in the polybutylene adipate-terephthalate is preferably (60:40) to (40:60), and can be specifically 60:40, 55:45, 50:50, 45:55 or 40:60; the weight average molecular weight of the polybutylene adipate-terephthalate is preferably 150,000 to 250,000, and can be specifically 150,000, 155,000, 160,000, 165,000, 170,000, 175,000, 180,000, 185,000, 190,000, 195,000, 200,000, 205,000, 210,000, 215,000, 220,000, 225,000, 230,000, 235,000, 240,000, 245,000 or 250,000.

[0051] In the antistatic composite material provided by the present invention, based on 100 parts by weight of the raw material biomass powder for preparing the biomass carbon ball, the amount of the polybutylene adipate-terephthalate is preferably 100 to 400 parts by weight, specifically 100 parts by weight, 110 parts by weight, 120 parts by weight, 130 parts by weight, 140 parts by weight, 150 parts by weight, 160 parts by weight, 170 parts by weight, 180 parts by weight, 190 parts by weight. 300 parts by weight, 310 parts by weight, 320 parts by weight, 330 parts by weight, 340 parts by weight, 350 parts by weight, 360 parts by weight, 370 parts by weight, 380 parts by weight, 390 parts by weight or 400 parts by weight.

[0052] In the antistatic composite material provided by the present invention, the dispersant is preferably one or more of polyethylene wax, stearic acid, zinc stearate and calcium stearate, and the polyethylene wax is preferably polyethylene wax OA9. In one embodiment provided by the present invention, the dispersant is stearic acid and zinc stearate, and the mass ratio of stearic acid and zinc stearate is preferably 1: (0.5-2), and more preferably 1: 1. In one embodiment provided by the present invention, the dispersant is zinc stearate and calcium stearate, and the mass ratio of zinc stearate and calcium stearate is preferably 0.7: (0.5-1.5), and more preferably 0.7: 0.8. In one embodiment provided by the present invention, the dispersant is polyethylene wax and calcium stearate, and the mass ratio of polyethylene wax and calcium stearate is preferably 1: (0.5-2), and more preferably 1: 1.

[0053] In the antistatic composite material provided by the present invention, based on 100 parts by weight of the raw biomass powder for preparing the biomass carbon balls, the amount of the dispersant is preferably 0.5 to 2 parts by weight, specifically 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight or 2 parts by weight.

[0054] In the antistatic composite material provided by the present invention, the chain extender is preferably one or more of pyromellitic anhydride (PMDA), ethylene-methyl methacrylate copolymer (EMMA), styrene-glycidyl methacrylate copolymer and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane. In one embodiment provided by the present invention, the chain extender is pyromellitic anhydride and ethylene-methyl methacrylate copolymer, and the mass ratio of the pyromellitic anhydride and ethylene-methyl methacrylate copolymer is preferably 1: (0.5-2), and more preferably 1: 1. In one embodiment provided by the present invention, the chain extender is ethylene-methyl methacrylate copolymer and styrene-glycidyl methacrylate copolymer, and the mass ratio of the ethylene-methyl methacrylate copolymer and styrene-glycidyl methacrylate copolymer is preferably 0.2: (0.1-3), and more preferably 0.2: 0.15. In one embodiment provided by the present invention, the chain extender is ethylene-methyl methacrylate copolymer, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and styrene-glycidyl methacrylate copolymer, and the mass ratio of the ethylene-methyl methacrylate copolymer, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and styrene-glycidyl methacrylate copolymer is preferably 1:(0.5-2):(1-3), more preferably 1:1:2.

[0055] In the antistatic composite material provided by the present invention, based on 100 parts by weight of the raw material biomass powder for preparing the biomass carbon ball, the amount of the chain extender is preferably 0.2 to 0.4 parts by weight, specifically 0.2 parts by weight, 0.21 parts by weight, 0.22 parts by weight, 0.23 parts by weight, 0.24 parts by weight, 0.25 parts by weight, 0.26 parts by weight, 0.27 parts by weight, 0.28 parts by weight, 0.29 parts by weight, 0.3 parts by weight, 0.31 parts by weight, 0.32 parts by weight, 0.33 parts by weight, 0.34 parts by weight, 0.35 parts by weight, 0.36 parts by weight, 0.37 parts by weight, 0.38 parts by weight, 0.39 parts by weight or 0.4 parts by weight.

[0056] The present invention also provides a method for preparing the antistatic composite material described in the above technical solution, comprising the following steps:

[0057] The biomass carbon balls, polybutylene adipate-terephthalate, a dispersant and a chain extender are melt-blended to obtain an antistatic composite material.

[0058] In the method for preparing the antistatic composite material provided by the present invention, the specific types and usage ratios of the polybutylene adipate-terephthalate, dispersant and chain extender have been introduced in the foregoing text and will not be repeated here.

[0059] In the method for preparing an antistatic composite material provided by the present invention, before the melt blending, the biomass carbon balls, polybutylene adipate-terephthalate, dispersant and chain extender are preferably mixed evenly; the mixing speed is preferably 600-800 rpm, specifically 600 rpm, 650 rpm, 700 rpm, 750 rpm or 800 rpm; the mixing temperature is preferably 15-35°C, specifically 25°C (room temperature); the mixing time is preferably 10-30 min, specifically 10 min, 15 min, 20 min, 25 min or 30 min.

[0060] In the method for preparing an antistatic composite material provided by the present invention, the melt blending is preferably carried out in a screw extruder; the extrusion speed of the screw extruder is preferably 100 to 200 rpm, specifically 100 rpm, 110 rpm, 120 rpm, 130 rpm, 140 rpm, 150 rpm, 160 rpm, 170 rpm, 180 rpm, 190 rpm or 200 rpm; the blending section temperature of the screw extruder is preferably 160 to 180°C, specifically 160°C, 161°C, 162°C, 163°C, 164°C, ℃, 165 ℃, 166 ℃, 167 ℃, 168 ℃, 169 ℃, 170 ℃, 171 ℃, 172 ℃, 173 ℃, 174 ℃, 175 ℃, 176 ℃, 177 ℃, 178 ℃, 179 ℃ or 180 ℃; the extrusion section temperature of the screw extruder is preferably 150-170 ℃, specifically 150 ℃, 151 ℃, 152 ℃, 153 ℃, 154 ℃, 155 ℃, 156 ℃, 157 ℃, 158 ℃, 159 ℃, 160 ℃, 161 ℃, 162 ℃, 163 ℃, 164 ℃, 165 ℃, 165 ℃, 166 ℃, 167 ℃, 168 ℃, 169 ℃ or 170 ℃.

[0061] In the method for preparing the antistatic composite material provided by the present invention, after the melt blending is completed, the obtained material is preferably dried, and the drying method is preferably baking, and the drying temperature is preferably 60-80°C, specifically 60°C, 65°C, 70°C, 75°C or 80°C.

[0062] The biomass carbon balls, preparation methods thereof, antistatic composite materials and preparation methods thereof provided by the present invention have at least the following advantages:

[0063] 1) Using persulfate to promote biomass hydrolysis, accelerate the carbon ball conversion process, improve the conversion efficiency of carbon ball materials, simplify the process, and reduce costs; and the prepared carbon ball materials are reactively melt-blended with PBAT raw materials to prepare a composite material with better compatibility, thereby realizing the comprehensive utilization of agricultural and forestry wastes;

[0064] 2) The carbon ball material obtained according to the method of the present invention has high application value, a large number of hydrophilic groups remain on the surface of the carbon ball, and has good compatibility with the composite material prepared from the PBAT raw material, excellent mechanical properties, and can be applied to the fields of antistatic materials;

[0065] 3) Compared with the prior art, the technical solution provided by the present invention uses persulfate to catalyze the hydrothermal carbonization process, high-temperature calcination to promote the degree of carbonization, and polybasic organic acid to remove tar. The process is relatively simple and the whole process is safe and environmentally friendly.

[0066] 4) The technical solution provided by the present invention is simple and efficient, has high production efficiency, can be produced on a large scale, and provides a feasible solution for the comprehensive utilization of agricultural and forestry wastes.

[0067] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.

[0068] In the following examples and comparative examples of the present invention, the specific evaluation methods of the materials are as follows:

[0069] 1) Yield:

[0070] Use an analytical balance to measure the weight of the biomass raw material and the prepared biomass carbon balls, calculate the yield, and then take the average value of multiple experiments.

[0071] 2) Microscopic morphology:

[0072] The prepared biomass carbon balls are carefully ground, the ground powder is placed in anhydrous ethanol for ultrasonic treatment, and then dropped onto a silicon wafer. After the alcohol evaporates, the silicon wafer is glued to the sample stage and its morphology is observed using a scanning electron microscope.

[0073] 3) Specific surface area:

[0074] The prepared biomass carbon balls were carefully ground, and the nitrogen adsorption and desorption amounts thereof were measured using a specific surface area analyzer to obtain the specific surface area data of the biomass carbon balls.

[0075] 4) Area resistance:

[0076] The composite material was compression molded at 180°C and 10 MPa for 10 min, and cooled under pressure to obtain a sheet with a specification of 120 mm×100 mm×2 mm. The area resistivity of the composite material was measured at room temperature using a high resistance meter. Five groups were tested in parallel and the result was taken as the average of the five groups of data.

[0077] 5) Tensile properties:

[0078] The composite material was compression molded at 180°C and 10 MPa for 10 min, cooled under pressure to obtain a 1 mm sheet, which was then cut into a dumbbell shape of 20 mm × 4 mm × 1 mm and tested using a universal tensile testing machine in accordance with ASTM D63-2014 at a tensile speed of 50 mm / min. Five groups of measurements were taken in parallel, and the average value of the five groups of data was taken.

[0079] Example 1

[0080] First, 100 parts by weight of 400-mesh sunflower seed shell powder, 200 parts by weight of ammonium persulfate and 2000 parts by weight of deionized water were placed in a high-pressure reactor for hydrothermal reaction for 12 hours at a hydrothermal reaction temperature of 220°C. After the reaction, the mixture was quickly filtered with a vacuum filter and repeatedly washed with deionized water until the upper liquid changed from black to colorless. The washed product was placed in an oven and dried at 60°C to obtain a dried material. The dried material was then placed in a high-temperature pure argon atmosphere furnace and heated to 500°C at a heating rate of 5°C / min. ℃, calcine at a constant temperature for 60min, and then cool to room temperature at a rate of 5℃ / min to obtain a pyrolysis material; then place the pyrolysis material, 20 parts by weight of citric acid and 400 parts by weight of anhydrous ethanol in a large beaker, and react in an ultrasonic machine in a water bath for 20min, the ultrasonic frequency is 40KHz, and the water bath temperature is 60℃; finally, use a vacuum filter to quickly filter, repeatedly wash with deionized water, place the washed product in an oven at 60℃ to dry, and then grind it to 800 mesh in a ball mill; weigh the mass of the obtained biomass carbon balls and record it.

[0081] The above-mentioned biomass carbon ball powder is placed in a high-speed mixer, 400 parts by weight of PBAT with a weight average molecular weight of 150,000 (the molar ratio of BA to BT in PBAT is 60:40) is added, and then 0.5 parts by weight of polyethylene wax OA9 and 0.2 parts by weight of pyromellitic anhydride are added, and mixed at room temperature for 10 minutes, and the speed is set to 600 rpm; then the mixed materials are melt-blended and extruded into granules in a twin-screw extruder, the blending temperature is set to 160°C, the extrusion temperature is set to 150°C, and the screw extrusion speed is 100 rpm; finally, the obtained pellets are dried at 60°C to obtain a biomass carbon ball / PBAT antistatic composite material.

[0082] Scanning electron microscope images of biomass carbon balls Figure 1 As shown, without gold spraying, the picture is clear and bright, indicating strong conductivity, and the morphology is carbon spheres of different sizes, indicating a high conversion rate of carbon spheres.

[0083] After testing, the yield of biomass carbon balls was 10.2% and the specific surface area was 284.54m2 g -1 ; The area resistance of the composite material is 9.73×10 7 Ω / sq., and the tensile properties are shown in Table 1.

[0084] Example 2

[0085] First, 100 parts by weight of 450-mesh rice straw powder, 250 parts by weight of potassium persulfate and 2000 parts by weight of deionized water were placed in a high-pressure reactor for hydrothermal reaction for 15 hours at a hydrothermal reaction temperature of 225°C. After the reaction, the mixture was quickly filtered with a vacuum filter and repeatedly washed with deionized water until the upper liquid changed from black to colorless. The washed product was placed in an oven and dried at 65°C to obtain a dried material. The dried material was then placed in a high-temperature pure argon atmosphere furnace and heated to 525°C at a heating rate of 6°C / min. ℃, calcine at a constant temperature for 70min, and then cool to room temperature at a rate of 6℃ / min to obtain a pyrolysis material; then place the pyrolysis material, 22 parts by weight of tartaric acid and 400 parts by weight of anhydrous ethanol in a large beaker, and react in an ultrasonic machine in a water bath for 25min, the ultrasonic frequency is 45KHz, and the water bath temperature is 65℃; finally, use a vacuum filter to quickly filter, repeatedly wash with deionized water, place the washed product in an oven at 65℃ to dry, and then grind it to 850 mesh in a ball mill; weigh the mass of the obtained biomass carbon balls and record it.

[0086] The above-mentioned biomass carbon ball powder is placed in a high-speed mixer, 300 parts by weight of PBAT with a weight average molecular weight of 170,000 (the molar ratio of BA to BT in PBAT is 55:45) is added, and then 0.8 parts by weight of stearic acid and 0.25 parts by weight of ethylene-methyl methacrylate copolymer with a weight average molecular weight of 25,000 (the molar ratio of ethylene repeating units to methyl methacrylate repeating units is 4:1) are added, and mixed at room temperature for 15 minutes, and the speed is set to 650 rpm; then the mixed materials are melt-blended and extruded into granules in a twin-screw extruder, the blending temperature is set to 165°C, the extrusion temperature is set to 155°C, and the screw extrusion speed is 125 rpm; finally, the obtained pellets are dried at 65°C to obtain a biomass carbon ball / PBAT antistatic composite material.

[0087] After testing, the yield of biomass carbon balls was 10.5% and the specific surface area was 303.27m 2 g -1 ; The area resistance of the composite material is 2.79×10 7 Ω / sq., and the tensile properties are shown in Table 1.

[0088] Example 3

[0089] First, 50 parts by weight of 500-mesh rice husk powder, 50 parts by weight of 500-mesh corn stalk powder, 300 parts by weight of sodium persulfate and 2000 parts by weight of deionized water were placed in a high-pressure reactor for hydrothermal reaction for 18 hours at a hydrothermal reaction temperature of 230°C. After the reaction, the mixture was quickly filtered with a vacuum filter and repeatedly washed with deionized water until the upper liquid changed from black to colorless. The washed product was placed in an oven and dried at 70°C to obtain a dried material. The dried material was then placed in a high-temperature pure argon atmosphere furnace and heated at a rate of 7°C / min. The temperature was raised to 550°C, calcined at a constant temperature for 70 minutes, and then cooled to room temperature at a rate of 7°C / min to obtain a pyrolysis material; the pyrolysis material, 25 parts by weight of malic acid and 400 parts by weight of anhydrous ethanol were placed in a large beaker, and reacted in an ultrasonic machine in a water bath for 30 minutes, with an ultrasonic frequency of 50KHz and a water bath temperature of 70°C; finally, a vacuum filter was used for rapid filtration, and the product was repeatedly washed with deionized water, and the washed product was placed in an oven to dry at 70°C, and then ground to 900 mesh in a ball mill; the mass of the obtained biomass carbon balls was weighed and recorded.

[0090] The above-mentioned biomass carbon ball powder is placed in a high-speed mixer, 200 parts by weight of PBAT with a weight average molecular weight of 200,000 (the molar ratio of BA to BT in PBAT is 50:50) is added, and then 0.6 parts by weight of stearic acid, 0.6 parts by weight of zinc stearate, 0.15 parts by weight of pyromellitic anhydride, 0.15 parts by weight of ethylene-methyl methacrylate copolymer with a weight average molecular weight of 25,000 (the molar ratio of ethylene repeating units to methyl methacrylate repeating units is 4:1) are added, and mixed at room temperature for 20 minutes, and the speed is set to 700 rpm; then the mixed materials are melt-blended and extruded in a twin-screw extruder for granulation, the blending temperature is set to 170°C, the extrusion temperature is set to 160°C, and the screw extrusion speed is 150 rpm; finally, the obtained pellets are dried at 70°C to obtain a biomass carbon ball / PBAT antistatic composite material.

[0091] The test showed that the yield of biomass carbon balls was 10.8% and the specific surface area was 359.25m 2 g -1 ; The area resistance of the composite material is 3.15×10 6 Ω / sq., and the tensile properties are shown in Table 1.

[0092] Example 4

[0093] First, 50 parts by weight of 550-mesh sisal powder, 50 parts by weight of 550-mesh jute powder, 200 parts by weight of ammonium persulfate, 150 parts by weight of potassium persulfate and 2000 parts by weight of deionized water were placed in a high-pressure reactor for hydrothermal reaction for 21 hours at a hydrothermal reaction temperature of 235°C. After the reaction, the mixture was quickly filtered with a vacuum filter and repeatedly washed with deionized water until the upper layer of liquid changed from black to colorless. The washed product was placed in an oven and dried at 75°C to obtain a dried material. The dried material was then placed in a high-temperature pure argon atmosphere furnace and heated at a heating rate of 9°C / min. The temperature was raised to 575°C, calcined at a constant temperature for 90 minutes, and then cooled to room temperature at a rate of 9°C / min to obtain a pyrolysis material; the pyrolysis material, 12 parts by weight of malic acid, 13 parts by weight of salicylic acid and 400 parts by weight of anhydrous ethanol were placed in a large beaker, and reacted in an ultrasonic machine in a water bath for 35 minutes, with an ultrasonic frequency of 55KHz and a water bath temperature of 75°C; finally, a vacuum filter was used for rapid filtration, and the product was repeatedly washed with deionized water, and the washed product was placed in an oven to dry at 75°C, and then ground to 900 mesh in a ball mill; the mass of the obtained biomass carbon balls was weighed and recorded.

[0094] The above-mentioned biomass carbon ball powder was placed in a high-speed mixer, and 150 parts by weight of PBAT with a weight average molecular weight of 220,000 (the molar ratio of BA to BT in PBAT is 45:55) was added, and then 0.7 parts by weight of zinc stearate, 0.8 parts by weight of calcium stearate, 0.2 parts by weight of ethylene-methyl methacrylate copolymer with a weight average molecular weight of 25,000 (the molar ratio of ethylene repeating units to methyl methacrylate repeating units is 4:1) was added, and 0.15 parts by weight of styrene with a weight average molecular weight of 18,000 was added. The mixture was prepared by mixing styrene-glycidyl methacrylate copolymer (the molar ratio of styrene repeating unit to glycidyl methacrylate repeating unit is 5:1) at room temperature for 25 minutes, and the rotation speed was set to 750 rpm; then the mixed materials were melt-blended and extruded into granules in a twin-screw extruder, the blending temperature was set to 175°C, the extrusion temperature was set to 165°C, and the screw extrusion speed was 175 rpm; finally, the obtained pellets were dried at 75°C to obtain a biomass carbon ball / PBAT antistatic composite material.

[0095] The test showed that the yield of biomass carbon balls was 11.0% and the specific surface area was 287.96m 2 g -1 ; The area resistance of the composite material is 5.65×10 5 Ω / sq., and the tensile properties are shown in Table 1.

[0096] Example 5

[0097] First, 30 parts by weight of 600-mesh sunflower seed shell powder, 30 parts by weight of 600-mesh peanut shell powder, 40 parts by weight of 600-mesh coconut shell powder, 200 parts by weight of potassium persulfate, 200 parts by weight of sodium persulfate and 2000 parts by weight of deionized water were placed in a high-pressure reactor for hydrothermal reaction for 24 hours at a hydrothermal reaction temperature of 240°C. After the reaction, the mixture was quickly filtered with a vacuum filter and repeatedly washed with deionized water until the upper layer of liquid changed from black to colorless. The washed product was placed in an oven and dried at 80°C to obtain a dried material. The dried material was then placed in a high-temperature pure argon atmosphere furnace and heated at a temperature of 10°C / min. The temperature was raised to 600°C, calcined at a constant temperature for 100 min, and then cooled to room temperature at a rate of 10°C / min to obtain a pyrolysis material; the pyrolysis material, 10 parts by weight of citric acid, 10 parts by weight of salicylic acid, 10 parts by weight of alginate and 400 parts by weight of anhydrous ethanol were placed in a large beaker, and reacted in an ultrasonic machine in a water bath for 40 min, with an ultrasonic frequency of 60 KHz and a water bath temperature of 80°C; finally, a vacuum filter was used for rapid filtration, and the product was repeatedly washed with deionized water, and the washed product was placed in an oven to dry at 80°C, and then ground to 1000 mesh in a ball mill; the mass of the obtained biomass carbon balls was weighed and recorded.

[0098] The above-mentioned biomass carbon ball powder is placed in a high-speed mixer, and 100 parts by weight of PBAT with a weight average molecular weight of 250,000 (the molar ratio of BA to BT in PBAT is 40:60) is added, and then 1 part by weight of polyethylene wax OA9, 1 part by weight of calcium stearate, 0.1 part by weight of ethylene-methyl methacrylate copolymer with a weight average molecular weight of 25,000 (the molar ratio of ethylene repeating units to methyl methacrylate repeating units is 4:1) is added, 0.1 part by weight of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and 0.2 part by weight of The mixture was mixed at room temperature for 30 minutes with a speed of 800 rpm. The mixed materials were melt-blended and extruded into granules in a twin-screw extruder, the blending temperature was set to 180°C, the extrusion temperature was set to 170°C, and the screw extrusion speed was 200 rpm. Finally, the pellets were dried at 80°C to obtain a biomass carbon ball / PBAT antistatic composite material.

[0099] The test showed that the yield of biomass carbon balls was 11.0% and the specific surface area was 349.81m 2 g -1 The area resistance of the composite material is 1.59×10 5 Ω / sq., and the tensile properties are shown in Table 1.

[0100] Comparative Example 1

[0101] First, take 100 parts by weight of 400-mesh sunflower seed shell powder and 2000 parts by weight of deionized water, place them in a high-pressure reactor for hydrothermal reaction for 12 hours, and the hydrothermal reaction temperature is 220°C; after the reaction, use a vacuum filter to quickly filter, wash repeatedly with deionized water until the upper liquid changes from black to colorless, and place the washed product in an oven at 60°C to dry to obtain a dried material; then place the dried material and 400 parts by weight of anhydrous ethanol in a large beaker, and treat it in an ultrasonic machine in a water bath for 20 minutes, with an ultrasonic frequency of 40KHz and a water bath temperature of 60°C; finally, use a vacuum filter to quickly filter, wash repeatedly with deionized water, place the washed product in an oven at 60°C to dry, and then grind it to 800 mesh in a ball mill; weigh the mass of the obtained biomass carbon material and record it.

[0102] The above-mentioned biomass carbon material is placed in a high-speed mixer, 400 parts by weight of PBAT with a weight average molecular weight of 150,000 (the molar ratio of BA to BT in PBAT is 60:40) is added, and then 0.5 parts by weight of polyethylene wax OA9 and 0.2 parts by weight of pyromellitic anhydride are added, and mixed at room temperature for 10 minutes, and the speed is set to 600 rpm; then the mixed materials are melt-blended and extruded into granules in a twin-screw extruder, the blending temperature is set to 160°C, the extrusion temperature is set to 150°C, and the screw extrusion speed is 100 rpm; finally, the obtained pellets are dried at 60°C to obtain a biomass carbon / PBAT composite material.

[0103] The prepared biomass carbon material is still dark brown, indicating that the reaction is not complete and the yield of the carbon material cannot be calculated. The scanning electron microscope image of the biomass carbon material is as follows: Figure 2 As shown, without gold spraying, the picture is blurred, indicating poor conductivity, and the morphology is mostly carbon blocks, indicating that the carbon ball conversion rate is low.

[0104] After testing, the specific surface area of ​​biomass carbon material is 104.15m 2 g -1 ; The area resistance of the composite material is 8.24×10 8 Ω / sq., and the tensile properties are shown in Table 1.

[0105] Comparative Example 2

[0106] First, 100 parts by weight of 400-mesh sunflower seed shell powder and 2000 parts by weight of deionized water were placed in a high-pressure reactor for hydrothermal reaction for 12 hours at a hydrothermal reaction temperature of 220°C. After the reaction, the powder was quickly filtered with a vacuum filter and repeatedly washed with deionized water until the upper liquid changed from black to colorless. The washed product was placed in an oven and dried at 60°C to obtain a dried material. The dried material was then placed in a high-temperature pure argon atmosphere furnace, heated to 500°C at a heating rate of 5°C / min, calcined at a constant temperature for 60 minutes, and then cooled to room temperature at a cooling rate of 5°C / min to obtain a pyrolysis material. The powder was then repeatedly washed with deionized water, the washed product was placed in an oven and dried at 60°C, and then ground to 800 mesh in a ball mill. The mass of the obtained biomass carbon material was weighed and recorded.

[0107] The above-mentioned biomass carbon material is placed in a high-speed mixer, 400 parts by weight of PBAT with a weight average molecular weight of 150,000 (the molar ratio of BA to BT in PBAT is 60:40) is added, and then 0.5 parts by weight of polyethylene wax OA9 and 0.2 parts by weight of pyromellitic anhydride are added, and mixed at room temperature for 10 minutes, and the speed is set to 600 rpm; then the mixed materials are melt-blended and extruded into granules in a twin-screw extruder, the blending temperature is set to 160°C, the extrusion temperature is set to 150°C, and the screw extrusion speed is 100 rpm; finally, the obtained pellets are dried at 60°C to obtain a biomass carbon / PBAT composite material.

[0108] After testing, the yield of biomass carbon material is 2.2%, and the specific surface area of ​​biomass carbon material is 185.97m 2 g -1 ; The area resistance of the composite material is 2.19×10 8 Ω / sq., and the tensile properties are shown in Table 1.

[0109] Comparative Example 3

[0110] The weight average molecular weight of PBAT raw material is 150,000, and the molar ratio of BA to BT in PBAT is 60:40. After testing, the area resistance of PBAT raw material is 1.27×10 9 Ω / sq., and the tensile properties are shown in Table 1.

[0111] Table 1 Test results of tensile properties of composite materials of different embodiments and comparative examples

[0112] sample Yield strength / MPa Breaking strength / MPa Elongation at break / % Example 1 24.5 11.5 802.4 Example 2 25.6 12.2 775.9 Example 3 26.3 14.1 726.1 Example 4 25.3 15.4 703.5 Example 5 23.9 15.1 657.7 Comparative Example 1 22.3 10.7 701.5 Comparative Example 2 22.9 11.2 739.6 Comparative Example 3 21.2 9.8 692.2

[0113] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A biomass carbon ball, which is prepared by hydrothermal reaction of biomass powder and persulfate, followed by washing, drying and oxygen-free calcination, ultrasonic reaction with organic acid in an organic solvent, and subsequent washing, drying and grinding; The organic acid is one or more of citric acid, tartaric acid, malic acid, salicylic acid, alginic acid and quinic acid; Based on 100 parts by weight of the biomass powder, the amount of the persulfate is 200 to 400 parts by weight, and the amount of the organic acid is 20 to 30 parts by weight.

2. The biomass carbon ball according to claim 1, characterized in that: The biomass powder is one or more of sunflower seed shell powder, sunflower stem powder, rice straw powder, rice husk powder, corn straw powder, sisal powder, jute powder, peanut shell powder, fir bark powder, pine cone powder, bamboo shoot shell powder, coconut shell powder, nut shell powder and soybean pod powder.

3. The biomass carbon ball according to claim 1, characterized in that: The persulfate is one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

4. A method for preparing biomass carbon balls according to any one of claims 1 to 3, comprising the following steps: a) subjecting biomass powder and persulfate to a hydrothermal reaction; after the reaction is completed, washing and drying the reaction product to obtain a dried material; b) calcining the dried material in the absence of oxygen to obtain a pyrolysis material; c) mixing the pyrolysis material with an organic acid in an organic solvent and subjecting the mixture to ultrasonic reaction; after the reaction is completed, washing, drying and grinding the reaction product to obtain biomass carbon balls.

5. The preparation method according to claim 4, characterized in that: In step a), the temperature of the hydrothermal reaction is 220-240° C.; the time of the hydrothermal reaction is 12-24 hours; In step b), the temperature of the oxygen-free calcination is 500-600° C.; the time of the oxygen-free calcination is 60-100 min; In step c), the ultrasonic frequency of the ultrasonic reaction is 40-60 KHz; the temperature of the ultrasonic reaction is 60-80° C.; and the time of the ultrasonic reaction is 20-40 min.

6. An antistatic composite material, prepared by melt blending raw materials, wherein the raw materials include biomass carbon balls, polybutylene adipate-terephthalate, a dispersant and a chain extender; The biomass carbon ball is the biomass carbon ball described in any one of claims 1 to 3 or the biomass carbon ball prepared by the preparation method described in any one of claims 4 to 5.

7. A method for preparing the antistatic composite material according to claim 6, comprising the following steps: The biomass carbon balls, polybutylene adipate-terephthalate, a dispersant and a chain extender are melt-blended to obtain an antistatic composite material.

8. The preparation method according to claim 7, characterized in that: The melt blending is carried out in a screw extruder; the extrusion speed of the screw extruder is 100-200 rpm; the blending section temperature of the screw extruder is 160-180°C; the extrusion section temperature of the screw extruder is 150-170°C.

Citation Information

Patent Citations

  • Novel method of preparing biomass based nano carbon black

    CN102190909A

  • Method for preparing biomass carbon by utilizing agricultural and forestry waste

    CN102583311A

  • Low temperature hydrothermal preparation method of biomass carbon microsphere / nanosphere

    CN104649246A

  • Method for preparing carbon microspheres through hydrothermal carbonization of biomass

    CN104671229A

  • Carbon material for adsorbing butanol and preparation method and application of carbon material

    CN105617992A