Grease composition and preparation method thereof, and application of pyrimidine compound and fatty alcohol

By adding pyrimidine compounds and fatty alcohols to the grease, a composition with high shear stability and colloid stability properties is solved, and the shortcomings of bentonite grease in these two aspects are achieved, and better high-temperature performance and rust prevention are achieved. Effect.

CN116042288BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111264953.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-11-12
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

The existing bentonite grease has shortcomings in shear stability and colloid stability, which is difficult to meet the needs of efficient lubrication and rust prevention.

Method used

Using a grease composition including pyrimidine compounds and fatty alcohols, the base oil, thickener, pyrimidine compounds, fatty alcohols and other additives are mixed and heat-raising refined to form a lubricating with high shear stability and colloid stability properties. fat.

Benefits of technology

It significantly improves the shear stability and colloid stability of the grease, and also has good high-temperature performance and anti-rust performance, shortens the grease formation time and improves the preparation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The present invention relates to the field of lubricating grease, and discloses a lubricating grease composition and a preparation method thereof, and applications of pyrimidine compounds and fatty alcohols. The lubricating grease composition comprises a base oil, a thickener and an additive, wherein the additive comprises a pyrimidine compound and a fatty alcohol, and the total content of the pyrimidine compound and the fatty alcohol is 0.1-1% by weight based on the total weight of the lubricating grease composition. The lubricating grease prepared by the lubricating grease composition has high shear stability and colloid stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lubricating grease, and in particular to a lubricating grease composition and a preparation method thereof, and applications of pyrimidine compounds and fatty alcohols. Background Art

[0002] Bentonite grease is an important type of non-soap high-temperature grease obtained by thickening lubricating oil base oil with organic modified bentonite. Bentonite grease is widely used in the lubrication of aircraft, automobiles, metallurgical equipment, heavy-load equipment, etc. due to its high dropping point or even no dropping point, relatively simple preparation process, even no need for heating, and low cost.

[0003] In 1943, Jordan prepared bentonite grease for the first time. In recent years, scholars at home and abroad have conducted extensive research on bentonite grease. CN1504552A uses vegetable oil as base oil, bentonite as thickener, amines or amines and phenols mixed antioxidants to prepare a biodegradable grease that meets environmental protection requirements; CN1197107A uses polyalphaolefin as base oil, phenyl-β-naphthylamine and diisooctyl diphenylamine as antioxidants and adds rust inhibitors (benzotriazole and sodium sebacate), extreme pressure agents (polytetrafluoroethylene and melamine cyanurate salt), and dispersants (acetone or 1,2-propylene glycol carbonate) to prepare a bentonite grease for aviation. The grease has good high and low temperature resistance, compatibility with rubber parts, and outstanding antioxidant and extreme pressure properties; CN101886017A A bentonite grease is prepared by using furfural refined oil, and an antioxidant and a pigment are added to the grease, so that the bentonite has good oxidation stability and corrosion resistance, and the addition of the pigment can give the product a special appearance and assist in distinguishing the types of grease; CN101240208A improves the process, including heating the bentonite suspension to 90-100°C, adding phosphoric acid to acidify the bentonite, adding a covering agent, a rust inhibitor (a mixture of treated sodium sulfonate and sodium nitrite), and adding a certain amount of wetting agent. The prepared bentonite grease has made great progress in thickening ability and rust resistance, and its water resistance has also been improved.

[0004] Current research and reports mainly focus on the formulation, production process and some properties of grease, but the research on its shear stability and colloid stability is insufficient. Therefore, there is still a lot of room for improvement in the shear stability and colloid stability of grease. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide a grease composition and a preparation method thereof and the application of pyrimidine compounds and fatty alcohols. The grease composition has high shear stability and colloid stability.

[0006] In order to achieve the above-mentioned purpose, the present invention provides a grease composition on one hand, which comprises a base oil, a thickener and an additive, wherein the additive comprises a pyrimidine compound and a fatty alcohol, and the total content of the pyrimidine compound and the fatty alcohol is 0.1-1% by weight based on the total weight of the grease composition.

[0007] The second aspect of the present invention provides a method for preparing a grease composition, which comprises: mixing a base oil, a thickener, a pyrimidine compound, a fatty alcohol and an optional dispersant, refining the mixture at a high temperature, and then mixing the mixture with other additives, wherein the total content of the pyrimidine compound and the fatty alcohol is 0.1-1% by weight.

[0008] A third aspect of the present invention provides the use of pyrimidine compounds and fatty alcohols in improving the shear stability and colloid stability of grease.

[0009] The grease composition of the present invention has high shear stability and colloid stability, as well as good high temperature performance and rust prevention performance. In addition, the preparation method provided by the present invention has a short grease formation time and high efficiency. DETAILED DESCRIPTION

[0010] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0011] In the present invention, the "shear stability" refers to the ability of grease to resist viscosity changes under mechanical shear force under certain conditions, and is an important indicator for evaluating the mechanical stability of grease. "Colloid stability" refers to the ability of grease to maintain a stable colloidal structure and prevent base oil from precipitating under heat and pressure conditions.

[0012] In a first aspect, the present invention provides a grease composition, which comprises a base oil, a thickener and an additive, wherein the additive comprises a pyrimidine compound and a fatty alcohol, and the total content of the pyrimidine compound and the fatty alcohol is 0.1-1 wt % based on the total weight of the grease composition.

[0013] The inventors of the present invention have found in their research that when the pyrimidine compounds and fatty alcohols as described above are used, the shear stability and colloidal stability of the grease can be greatly improved.

[0014] According to the present invention, in order to further improve the shear stability and colloid stability of the grease, preferably, based on the total weight of the grease composition, the total content of the pyrimidine compounds and fatty alcohols is 0.38-0.8 wt% (0.38 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%).

[0015] According to the present invention, preferably, the weight ratio of the pyrimidine compound to the fatty alcohol is 0.8-3, more preferably 1-2.5.

[0016] According to the present invention, preferably, the pyrimidine compound is selected from at least one of the compounds shown in Formula I, wherein R1, R2, R3 and R4 are independently selected from hydrogen, halogen, aromatic group or alkyl substituted or unsubstituted methoxy. Among them, the halogen can be F, Cl, Br or I; the aromatic group can be phenyl or alkyl substituted phenyl; the alkyl group can be C1-C6 alkyl (straight chain, branched chain, cyclic), including but not limited to methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, cyclopropyl, methylcyclopropyl, ethylcyclopropyl, cyclopentyl, methylcyclopentyl, cyclohexyl...etc.

[0017] More preferably, R1 is selected from halogen, phenylmethoxy or methoxy, R2 is selected from halogen or hydrogen, R3 is selected from hydrogen, methoxy or phenylmethoxy, and R4 is selected from hydrogen or methoxy.

[0018]

[0019] The pyrimidine compound is further preferably at least one of 5-bromo-2-methoxypyrimidine, 6-chloro-2,4-dimethoxypyrimidine and 5-bromo-4-(3-methoxyphenyl)pyrimidine.

[0020] According to the present invention, preferably, the fatty alcohol is selected from at least one of C12-C20 fatty alcohols, preferably at least one of (n-) dodecanol, (n-) tetradecanol, (n-) hexadecanol, (n-) octadecyl alcohol and (n-) eicosanol.

[0021] The inventors of the present invention have further discovered in their research that when the pyrimidine compounds or fatty alcohols or the content ranges as described above are used, the shear stability and colloid stability of the grease can be further improved.

[0022] According to the present invention, preferably, based on the total weight of the grease composition, the content of the base oil is 75-92 weight % (for example, it may be 75 weight %, 78 weight %, 80 weight %, 82 weight %, 84 weight %, 85 weight %, 86 weight %, 88 weight %, 90 weight %, 92 weight %), and more preferably 79-84.5 weight %.

[0023] According to the present invention, preferably, the kinematic viscosity of the base oil at 100°C is 5-40 mm 2 / s (for example, it can be 5mm 2 / s,6mm 2 / s,10mm 2 / s,15mm 2 / s,20mm 2 / s,25mm 2 / s, 30mm 2 / s, 35mm 2 / s, 40mm 2 / s, 45mm 2 / s,50mm 2 / s), more preferably 6-30mm 2 / s. It can be understood that the kinematic viscosity is a measure of the resistance to flow of a fluid under gravity, and refers to the distance that a fluid flows through a capillary in a calibrated kinematic viscometer per second under gravity at a fixed temperature. The kinematic viscosity test method is GB / T 30515.

[0024] According to the present invention, preferably, the base oil is selected from mineral base oil and / or synthetic base oil; more preferably, the mineral base oil is selected from at least one of low-sulfur paraffinic crude oil base oil (for example, 650SN base oil, 150BS base oil), low-sulfur intermediate base oil, cycloalkyl crude oil base oil and hydrogenated base oil (for example, 500N base oil); the synthetic oil is selected from at least one of synthetic hydrocarbon oil, ester oil, ether oil, silicone oil and fluoro oil; more preferably, the synthetic hydrocarbon oil is selected from poly α-olefin oil (PAO) and / or polybutene, the ester oil is selected from diesters such as dioctyl sebacate and / or polyol esters, and the ether oil is selected from alkyl diphenyl ether and / or polypropylene glycol.

[0025] According to the present invention, preferably, based on the total weight of the grease composition, the content of the thickener is 8-25 weight % (for example, 8 weight %, 10 weight %, 13 weight %, 15 weight %, 18 weight %, 20 weight %, 23 weight %, 25 weight %), and more preferably 9-17.5 weight %.

[0026] According to the present invention, preferably, the thickener is organic bentonite. The organic bentonite can be purchased commercially or prepared by itself. For example, the bentonite can be first modified into sodium bentonite, and then a covering agent is added, and after sufficient reaction, the covering agent is completely attached to the end surface of the bentonite grain structure, and then filtered, washed, dried, and crushed to obtain the organic bentonite.

[0027] According to the present invention, preferably, the grease composition further comprises at least one of a dispersant, an antioxidant and a rust inhibitor.

[0028] According to the present invention, preferably, based on the total weight of the grease composition, the content of the dispersant is 0.5-10 wt % (0.5 wt %, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt %, 6 wt %, 7 wt %, 8 wt %, 9 wt %, 10 wt %), more preferably 0.9-3 wt %.

[0029] According to the present invention, preferably, the dispersant is at least one of C1-C5 alcohol (monohydric alcohol or polyhydric alcohol), C1-C5 ketone and C1-C5 ester, preferably at least one of methanol, ethanol, ethylene glycol, glycerol, pentaerythritol, acetone and propylene carbonate.

[0030] According to the present invention, preferably, based on the total weight of the grease composition, the content of the antioxidant is 0.1-10 wt % (0.1 wt %, 1 wt %, 3 wt %, 5 wt %, 8 wt %, 10 wt %), more preferably 0.4-2 wt %.

[0031] According to the present invention, preferably, the antioxidant is a phenolic antioxidant, more preferably at least one of 2,6-di-tert-butyl-p-cresol, 2-naphthol, 2,6-di-tert-butyl-α-dimethylamino-p-cresol, 4,4-methylenebis(2,6-di-tert-butylphenol) and 2,6-di-tert-butyl-4-alkoxyphenol.

[0032] According to the present invention, preferably, based on the total weight of the grease composition, the content of the rust inhibitor is 0.1-10 wt % (for example, 0.1 wt %, 1 wt %, 3 wt %, 5 wt %, 8 wt %, 10 wt %), more preferably 0.4-1 wt %.

[0033] According to the present invention, preferably, the rust inhibitor is selected from sulfonate rust inhibitors, more preferably at least one of barium petroleum sulfonate, sodium petroleum sulfonate, barium dinonylnaphthalene sulfonate and zinc dinonylnaphthalene sulfonate.

[0034] According to the present invention, the grease composition consists only of the ingredients described above.

[0035] According to the present invention, a grease composition with better performance can be obtained by mixing preferred types of base oil, thickener, additives, dispersant, antioxidant and rust inhibitor in preferred proportions.

[0036] In a second aspect, the present invention provides a method for preparing a grease composition, the method comprising: mixing a base oil, a thickener, a pyrimidine compound, a fatty alcohol and an optional dispersant, refining the mixture at a high temperature, and then mixing the mixture with other additives, wherein the total content of the pyrimidine compound and the fatty alcohol is 0.1-1% by weight.

[0037] The inventors of the present invention have found that the grease composition prepared by this method not only has higher shear stability and colloid stability, but also the addition of the pyrimidine compounds and fatty alcohols in the early stage of grease preparation is more conducive to grease formation and greatly shortens the grease formation time.

[0038] Preferably, the method for preparing the grease composition comprises: mixing the base oil and the thickener, and stirring evenly, then adding the optional dispersant, and stirring evenly; heating to 100-120°C, and maintaining for 10-20 minutes; then adding other additives, stirring evenly, and then grinding the material into grease to obtain a finished product.

[0039] The grinding method may be a conventional method in the art, for example, grinding by a three-roll mill.

[0040] Those skilled in the art can obtain the amount of various raw materials used in the preparation method of the second aspect according to the content of the aforementioned base oil, thickener, dispersant and additives, which will not be described in detail here.

[0041] In a third aspect, the present invention provides the use of pyrimidine compounds and fatty alcohols in improving the shear stability and colloid stability of grease. The inventors of the present invention have found in their research that pyrimidine compounds and fatty alcohols can exert better shear stability and colloid stability in grease, especially bentonite grease.

[0042] Among them, the specific types and proportions of pyrimidine compounds and fatty alcohols are as described above and will not be repeated here.

[0043] According to a particularly preferred embodiment of the present invention, the grease composition is prepared according to the following components and methods:

[0044] Based on the total weight of the raw material components, the raw material components contain 77-80 weight % of 650SN base oil (belonging to low-sulfur paraffin-based crude oil base oil), 16.5-18 weight % of organic bentonite, 0.8-1.1 weight % of ethanol, 0.8-1.1 weight % of 2,6-di-tert-butyl-4-alkoxyphenol, 0.8-1.1 weight % of zinc dinonylnaphthalenesulfonate, and a total content of 0.38-0.45 weight % of 6-chloro-2,4-dimethoxypyrimidine and n-tetradecanol, wherein the weight ratio of 6-chloro-2,4-dimethoxypyrimidine to n-tetradecanol is 1-1.3.

[0045] The above-mentioned 650SN base oil, 6-chloro-2,4-dimethoxypyrimidine, n-tetradecanol and organic bentonite are mixed and stirred evenly, and then ethanol is added thereto and stirred rapidly until a grease structure is formed; the temperature is raised to 115-120°C and maintained for 10-13 minutes, 2,6-di-tert-butyl-4-alkoxyphenol and zinc dinonylnaphthalenesulfonate are added, and the mixture is cooled to room temperature and ground by a three-roll mill for 2-3 times to form grease.

[0046] The present invention will be described in detail below by way of examples. The performance evaluation in the following examples and comparative examples is carried out according to the following method:

[0047] The dropping point is determined using the GB / T 3498 method. The higher the measured value, the better the high temperature performance.

[0048] The cone penetration, 100,000 cone penetration and 60 cone penetration are measured using the GB / T 269 method. The smaller the value, the thicker the fat.

[0049] The colloid stability is characterized by the steel mesh oil separation index, and the steel mesh oil separation performance is measured using the NB / SH / T0324 method. The smaller the steel mesh oil separation performance value, the better the colloid stability.

[0050] GB / T 7326 method was used to determine the corrosion of copper sheets;

[0051] The corrosion resistance was determined using the GB / T 5018 method;

[0052] The shear stability is measured by the difference between 100,000 cone penetrations and 60 cone penetrations. The smaller the value, the better the shear stability.

[0053] The sources of the main raw materials used are shown in Table 1.

[0054] Table 1

[0055] Raw material name factory PAO6 (Poly α-olefin oil) ExxonMobil PAO10 (Poly α-olefin oil) ExxonMobil 650SN base oil (low sulfur paraffin-based crude oil base oil) Yanshan Petrochemical 500N base oil (hydrogenated base oil) Ssangyong 150BS base oil (low sulfur paraffin-based crude oil base oil) Tai Ao Star Co., Ltd. Organic bentonite Zhejiang Fenghong New Materials Co., Ltd. 5-Bromo-2-methoxypyrimidine Aladdin 6-Chloro-2,4-dimethoxypyrimidine Aladdin 5-Bromo-4-(3-methoxyphenyl)pyrimidine Aladdin Dodecanol Aladdin Tetradecanol Aladdin Cetyl Alcohol Aladdin Ethanol Longxi Technology Co., Ltd. Glycerol Longxi Technology Co., Ltd. acetone Longxi Technology Co., Ltd. Propylene carbonate Longxi Technology Co., Ltd.

[0056] Example 1

[0057] Raw material components: 500N base oil (100℃ kinematic viscosity is 10.5mm 2 / s) 90g, organic bentonite 10g, acetone 3g, 5-bromo-2-methoxypyrimidine 0.4g, n-dodecanol 0.4g; 2,6-di-tert-butyl-α-dimethylamino-p-cresol 2g, barium dinonylnaphthalenesulfonate 1g.

[0058] The above-mentioned 500N base oil, 5-bromo-2-methoxypyrimidine, n-dodecyl alcohol and organic bentonite are mixed and stirred evenly, and then acetone is added thereto and stirred rapidly until a grease structure is formed; the temperature is raised to 100°C and maintained for 20 minutes; after adding 2,6-di-tert-butyl-α-dimethylamino-p-cresol and barium dinonylnaphthalenesulfonate, the mixture is cooled to room temperature and ground twice by a three-roll mill to form grease.

[0059] Example 2

[0060] Raw material components: 650SN base oil (100℃ kinematic viscosity is 29.8mm 2 / s) 82g, organic bentonite 18g, ethanol 1g, 6-chloro-2,4-dimethoxypyrimidine 0.2g, n-tetradecanol 0.2g, and 2,6-di-tert-butyl-4-alkoxyphenol 1g, zinc dinonylnaphthalenesulfonate 1g.

[0061] The above-mentioned 650SN base oil, 6-chloro-2,4-dimethoxypyrimidine, n-tetradecanol and organic bentonite are mixed and stirred evenly, and then ethanol is added thereto and stirred rapidly until a grease structure is formed; the temperature is raised to 120°C and maintained for 10 minutes, 2,6-di-tert-butyl-4-alkoxyphenol and zinc dinonylnaphthalenesulfonate are added, and the mixture is cooled to room temperature and ground three times by a three-roll mill to form grease.

[0062] Example 3

[0063] Raw material components: PAO6 base oil (100℃ kinematic viscosity is 6.1mm 2 / s) 85g, organic bentonite 15g, glycerol 2g, 5-bromo-4-(3-methoxyphenyl) pyrimidine 0.3g, 0.2g n-hexadecanol, 2,6-di-tert-butyl-p-cresol 0.5g, and barium petroleum sulfonate 0.5g.

[0064] The above-mentioned PAO6 base oil, 5-bromo-4-(3-methoxyphenyl)pyrimidine, n-hexadecanol and organic bentonite are mixed and stirred evenly, and then propylene glycol is added thereto and stirred rapidly until a grease structure is formed; the temperature is raised to 110°C and maintained for 15 minutes, 2,6-di-tert-butyl-p-cresol and barium petroleum sulfonate are added, and the mixture is cooled to room temperature and ground three times on a three-roll mill to form grease.

[0065] Example 4

[0066] Raw material components: 650SN base oil (100℃ kinematic viscosity is 12.9mm 2 / s) 88g, organic bentonite 12g, propylene carbonate 2g, 5-bromo-4-(3-methoxyphenyl)pyrimidine 0.5g, n-octadecanol 0.2g, 2-naphthol 1g, sodium petroleum sulfonate 1g.

[0067] The above-mentioned 650SN base oil, 5-bromo-4-(3-methoxyphenyl)pyrimidine, n-octadecyl alcohol and organic bentonite are mixed and stirred evenly, and then propylene carbonate is added thereto and stirred rapidly until a grease structure is formed; the temperature is raised to 100°C and maintained for 10 minutes, 2-naphthol and 1 gram of sodium petroleum sulfonate are added, and the mixture is cooled to room temperature and ground twice by a three-roll mill to form a grease.

[0068] Example 5

[0069] Raw material components: PAO10 base oil 86g (100℃ kinematic viscosity is 10.2mm 2 / s), 8g of organic bentonite, 0.7g of acetone, 0.14g of 5-bromo-2-methoxypyrimidine, 0.16g of n-dodecanol, 3g of 2,6-di-tert-butyl-α-dimethylamino-p-cresol, and 2g of barium dinonylnaphthalenesulfonate.

[0070] The above-mentioned PAO10 base oil, 5-bromo-2-methoxypyrimidine, n-dodecyl alcohol and organic bentonite are mixed and stirred evenly, and then acetone is added thereto and stirred rapidly until a grease structure is formed; the temperature is raised to 100°C and maintained for 20 minutes; after adding 2,6-di-tert-butyl-α-dimethylamino-p-cresol and barium dinonylnaphthalenesulfonate, the mixture is cooled to room temperature and ground twice by a three-roll mill to form grease.

[0071] Example 6

[0072] Raw material components: 500N base oil 75g (100℃ kinematic viscosity is 10.5mm 2 / s), 18g of organic bentonite, 5.6g of acetone, 0.75g of 5-bromo-2-methoxypyrimidine, 0.25g of n-dodecanol, 0.2g of 2,6-di-tert-butyl-α-dimethylamino-p-cresol, and 0.2g of barium dinonylnaphthalenesulfonate.

[0073] The above-mentioned 500N base oil, 5-bromo-2-methoxypyrimidine, n-dodecyl alcohol and organic bentonite are mixed and stirred evenly, and then acetone is added thereto and stirred rapidly until a grease structure is formed; the temperature is raised to 100°C and maintained for 20 minutes; after adding 2,6-di-tert-butyl-α-dimethylamino-p-cresol and barium dinonylnaphthalenesulfonate, the mixture is cooled to room temperature and ground twice by a three-roll mill to form grease.

[0074] Example 7

[0075] Grease was prepared according to the method of Example 1, except that 0.35 g of 5-bromo-2-methoxypyrimidine and 0.44 g of n-dodecanol were used (ie, the weight ratio of 5-bromo-2-methoxypyrimidine to n-dodecanol was 0.8).

[0076] Example 8

[0077] Grease was prepared according to the method of Example 1, except that 0.6 g of 5-bromo-2-methoxypyrimidine and 0.2 g of n-dodecanol were used (ie, the weight ratio of 5-bromo-2-methoxypyrimidine to n-dodecanol was 3).

[0078] Comparative Example 1

[0079] Grease was prepared according to the method of Example 1, except that the amount of 5-bromo-2-methoxypyrimidine was 3 g and the amount of n-dodecanol was 1 g (i.e., based on the total weight of the grease composition, the total content of the pyrimidine compounds and the fatty alcohol was 3.6% by weight, and the weight ratio of the pyrimidine compounds to the fatty alcohol was 3).

[0080] Comparative Example 2

[0081] A grease was prepared according to the method of Example 1, except that 5-bromo-2-methoxypyrimidine was replaced by dodecylpyridinium chloride.

[0082] Comparative Example 3

[0083] The grease was prepared according to the method of Example 1, except that n-dodecyl alcohol was replaced by phenylethyl alcohol.

[0084] Comparative Example 4

[0085] Grease was prepared according to the method of Example 1, except that no pyrimidine compounds and fatty alcohols were added, and the missing 0.8 g of material due to the failure to add pyrimidine compounds and fatty alcohols was made up according to the ratio of 500N base oil, organic bentonite, acetone, 2,6-di-tert-butyl-α-dimethylamino-p-cresol, and barium dinonylnaphthalenesulfonate used in Example 1.

[0086] Test Example 1

[0087] For the greases prepared in Examples 1-8 and Comparative Examples 1-4, the dropping point, cone penetration, cone penetration 100,000 times, steel mesh oil separation performance, copper sheet corrosion, corrosion resistance, shear stability and colloid stability were measured respectively. The results are shown in Table 2.

[0088] Table 2

[0089]

[0090] It can be seen from the above results, especially the difference between 100,000 cone penetrations and 60 cone penetrations and the steel mesh oil separation index, that the grease composition prepared by the technical solution of the present invention has high shear stability and colloid stability. It also has good high temperature performance and rust prevention performance. It can be seen from Example 1 and Examples 5-6 that the grease prepared by the preferred, specific ratio of the composition of the present invention can have better shear stability and colloid stability.

[0091] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A grease composition, comprising a base oil, a thickener and an additive, characterized in that: The additive comprises a pyrimidine compound and a fatty alcohol, the total content of the pyrimidine compound and the fatty alcohol being 0.1-1% by weight based on the total weight of the grease composition, and the weight ratio of the pyrimidine compound to the fatty alcohol being 0.8-2.5; the fatty alcohol being at least one selected from the group consisting of C12-C20 fatty alcohols; Wherein, the pyrimidine compound is selected from at least one of the compounds represented by Formula I, wherein R1, R2, R3 and R4 are each independently selected from hydrogen, halogen, aromatic or alkyl-substituted or unsubstituted methoxy, and the alkyl group is selected from a C1-C6 alkyl group; Formula I.

2. The grease composition according to claim 1, wherein Based on the total weight of the grease composition, the total content of the pyrimidine compound and the fatty alcohol is 0.38-0.8% by weight; and / or, the weight ratio of the pyrimidine compound to the fatty alcohol is 1-2.5; And / or, R1 is selected from halogen, phenylmethoxy or methoxy, R2 is selected from halogen or hydrogen, R3 is selected from hydrogen, methoxy or phenylmethoxy, and R4 is selected from hydrogen or methoxy.

3. The grease composition according to claim 2, wherein The pyrimidine compound is selected from at least one of 5-bromo-2-methoxypyrimidine, 6-chloro-2,4-dimethoxypyrimidine and 5-bromo-4-(3-methoxyphenyl)pyrimidine; And / or, the fatty alcohol is selected from at least one of lauryl alcohol, tetradecanol, hexadecanol, stearyl alcohol and eicosanol.

4. The grease composition according to claim 1, wherein Based on the total weight of the grease composition, the content of the base oil is 75-92% by weight; And / or, the kinematic viscosity of the base oil at 100°C is 5-40 mm 2 / s; And / or, the base oil is selected from mineral base oil and / or synthetic base oil.

5. The grease composition according to claim 4, wherein Based on the total weight of the grease composition, the content of the base oil is 79-84.5% by weight; And / or, the kinematic viscosity of the base oil at 100°C is 6-30 mm 2 / s; And / or, the mineral base oil is selected from at least one of low-sulfur paraffin-based crude oil base oil, low-sulfur intermediate base oil, cycloalkane crude oil base oil and hydrogenated base oil; the synthetic base oil is selected from at least one of synthetic hydrocarbon oil, ester oil, ether oil, silicone oil and fluoro oil.

6. The grease composition according to claim 5, wherein The synthetic hydrocarbon oil is selected from poly-α-olefin oil and / or polybutene, the ester oil is selected from dioctyl sebacate and / or polyol ester, and the ether oil is selected from alkyl diphenyl ether and / or polypropylene glycol.

7. The grease composition according to claim 1, wherein Based on the total weight of the grease composition, the content of the thickener is 8-25% by weight; And / or, the thickener is organic bentonite.

8. The grease composition according to claim 7, wherein Based on the total weight of the grease composition, the content of the thickener is 9-17.5% by weight.

9. The grease composition according to claim 1, wherein The grease composition further includes at least one of a dispersant, an antioxidant and a rust inhibitor.

10. The grease composition according to claim 9, wherein Based on the total weight of the grease composition, the content of the dispersant is 0.5-10% by weight; And / or, the dispersant is at least one of C1-C5 alcohol, C1-C5 ketone and C1-C5 ester.

11. The grease composition according to claim 10, wherein Based on the total weight of the grease composition, the content of the dispersant is 0.9-3% by weight; And / or, the dispersant is at least one of methanol, ethanol, ethylene glycol, glycerol, pentaerythritol, acetone and propylene carbonate.

12. The grease composition according to claim 9, wherein Based on the total weight of the grease composition, the content of the antioxidant is 0.1-10% by weight; And / or, the antioxidant is a phenolic antioxidant.

13. The grease composition according to claim 12, wherein Based on the total weight of the grease composition, the content of the antioxidant is 0.4-2% by weight; And / or, the antioxidant is at least one of 2,6-di-tert-butyl-p-cresol, 2-naphthol, 2,6-di-tert-butyl-α-dimethylamino-p-cresol, 4,4-methylenebis(2,6-di-tert-butylphenol) and 2,6-di-tert-butyl-4-alkoxyphenol.

14. The grease composition according to claim 9, wherein Based on the total weight of the grease composition, the content of the rust inhibitor is 0.1-10% by weight; And / or, the rust inhibitor is selected from sulfonate rust inhibitors.

15. The grease composition according to claim 14, wherein Based on the total weight of the grease composition, the content of the rust inhibitor is 0.4-1% by weight; And / or, the rust inhibitor is selected from at least one of barium petroleum sulfonate, sodium petroleum sulfonate, barium dinonylnaphthalene sulfonate and zinc dinonylnaphthalene sulfonate.

16. A method for preparing a grease composition, characterized in that: The method comprises: mixing a base oil, a thickener, a pyrimidine compound, a fatty alcohol and an optional dispersant, heating and refining the mixture, and then mixing the mixture with other additives, wherein the total content of the pyrimidine compound and the fatty alcohol is 0.1-1% by weight, and the weight ratio of the pyrimidine compound to the fatty alcohol is 0.8-2.5; and the fatty alcohol is selected from at least one of the fatty alcohols of C12-C20; Wherein, the pyrimidine compound is selected from at least one of the compounds represented by Formula I, wherein R1, R2, R3 and R4 are each independently selected from hydrogen, halogen, aromatic or alkyl-substituted or unsubstituted methoxy, and the alkyl group is selected from a C1-C6 alkyl group; Formula I.

17. Application of pyrimidine compounds and fatty alcohols in improving the shear stability and colloid stability of grease, wherein: The pyrimidine compound is selected from at least one of the compounds shown in Formula I, wherein R1, R2, R3 and R4 are independently selected from hydrogen, halogen, aromatic group or alkyl substituted or unsubstituted methoxy, and the alkyl group is selected from C1-C6 alkyl; the fatty alcohol is selected from at least one of C12-C20 fatty alcohols; Formula I.