Method for preparing non-stick layer of metal cooking pot and detecting non-stick property by contact angle
By forming a micro-nano hydrophobic structure on the surface of the aluminum alloy pot embryo, the problem of decreasing bonding force caused by thermal expansion and contraction of the non-stick layer of the metal cooking pot is solved, and the non-stickness and wear resistance are improved, ensuring non-stickness and non-stickness are ensured. Stability and service life of the layer.
Patent Information
- Application Number
- CN202310022577.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-01-08
AI Technical Summary
Due to thermal expansion and contraction of metal cooking pots, the bonding force between the non-stick layer and the pot embryo body decreases, resulting in weakening of non-stickness and shortening of service life.
The integrated micro-nanohydrophobic structure is formed on the surface of the aluminum alloy pot embryo, and the oxide film is removed by shooting peening, acid etching is formed to form micro-pits, and constant flow anodization is used to form loose AlOOH film layer, and AlOOH is sprayed and heated on its surface. -SiO2 composite sol forms a continuous Al2O3-SiO2 particle structure.
The stable and integrated connection between the non-stick layer and the aluminum alloy pot embryo body is achieved, which improves the non-stickness and wear resistance, and ensures the stability and service life of the non-stick layer under high temperature conditions.
Smart Images

Figure CN116043303B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of non-stick properties of cooking pots, and in particular to a method for preparing a non-stick layer of a metal cooking pot and detecting the non-stick property through a contact angle. Background Art
[0002] Since the metal base material of metal cooking pots is treated with sandblasting technology, its roughness is less. After the cookware is used for a period of time, the bonding strength between the non-stick coating and the metal base material will decrease due to long-term thermal expansion and contraction, and the non-stick coating may even fall off during use.
[0003] The invention patent application CN110731685A discloses a spray coating process for a pot. After shot blasting, the bottom of the pot forms a fine wave crest and trough structure, which improves the adhesion of the non-stick coating and reduces the contact area between the non-stick coating and the spatula, reducing the risk of being shoveled off by the spatula and increasing its service life. It can be seen that the limited bonding force between the pot body and the coating makes it difficult to reduce the shedding of the coating and maintain the non-stick property of the cooker. Summary of the invention
[0004] The object of the present invention is to provide a metal cooking pot. The present invention forms a non-stick layer with an integral connection structure on the surface of an aluminum alloy pot body. The deformation of the non-stick layer and the aluminum alloy pot body are consistent, and the non-stick property is stable.
[0005] To solve this technical problem, the technical solution of the present invention is: a method for preparing a non-stick layer of a metal cooking pot, comprising the following steps:
[0006] S1. Shot peening the aluminum alloy pot embryo to remove the surface oxide film, cleaning and drying;
[0007] S2, spraying acid solution onto the surface of the pot embryo to etch and form a micron pit structure;
[0008] S3, subjecting the pot embryo body having a micron concave-convex structure obtained by surface etching to constant current anodizing;
[0009] S4, coating the surface of the loose AlOOH film layer with AlOOH-SiO2 composite sol, spraying it on the loose AlOOH film layer obtained in S3, drying it, and baking it;
[0010] S5. Heating. The AlOOH-SiO2 composite sol grows on the surface of the loose AlOOH film layer and in the gaps to become particles attached to the surface of the loose AlOOH film layer and in the gaps. The AlOOH-SiO2 particles and the AlOOH in the loose AlOOH film layer simultaneously lose water and are converted into Al2O3 during the heating process.
[0011] Preferably, the acid solution for etching in S2 is a mixture of H2SO4 and HF, and its composition is as follows:
[0012] H2SO4 concentration is 0.5 to 0.6 mol / L;
[0013] The HF concentration is 0.002 to 0.005 mol / L.
[0014] Preferably, the constant current anodization in S3 includes a start-up phase of 0V to 100V, a rising phase of voltage from 100V to 120V, and a constant voltage phase of 140V to 160V, and a loose AlOOH film layer is formed on the surface;
[0015] Constant current anodization is 30mA / cm 2 ;
[0016] The electrolyte is an aqueous solution of 0.2 mol / L oxalic acid;
[0017] The temperature of anodization is 6°C to 8°C.
[0018] Preferably, the viscosity of the AlOOH-SiO2 composite sol is 500 mPa·s to 1000 mPa·s.
[0019] The preferred spraying process of S4 is as follows:
[0020] AlOOH-SiO2 composite sol liquid is sprayed on the loose AlOOH film layer;
[0021] The spraying amount of AlOOH-SiO2 composite sol is 80g / m 2 Up to 120g / m 2 .
[0022] The preferred process conditions for heating in S5 are as follows:
[0023] The temperature is 500°C to 600°C; the time is 2 hours to 3 hours.
[0024] The preparation method of the AlOOH-SiO2 composite sol in S5 is preferably as follows:
[0025] The AlOOH sol and SiO2 sol prepared separately are mixed in a molar ratio of Al to Si of (2.1 to 3.3):1;
[0026] After aging at room temperature for 24 hours, AlOOH-SiO2 composite sol was obtained.
[0027] The preferred method for preparing the AlOOH-SiO2 composite sol comprises the following steps:
[0028] S11, mixing Al(OC3H7)3 with deionized water for hydrolysis, then adding HNO3 and stirring in a water bath to obtain AlOOH sol;
[0029] Wherein, the molar ratio of Al(OC3H7)3, deionized water and HNO3 is 1:(150 to 180):(0.3 to 0.6);
[0030] S12, adding ethyl orthosilicate and ethanol solution to the AlOOH sol obtained in S11, adding HNO3 to adjust the pH value to 3 to 4, and stirring to obtain a transparent and stable sol;
[0031] The molar ratio of ethyl orthosilicate to ethanol in S12 is 1:(18 to 20).
[0032] Another object of the present invention is to provide a method for detecting the non-stickiness of metal cooking pots by using the contact angle. The present invention directly detects the non-stickiness of metal cooking pots by using the contact angle of water, and the detection is direct and easy to operate.
[0033] To solve this technical problem, the technical solution of the present invention is: a method for detecting the non-stickiness of the metal cooking pot made by the present invention through contact angle, wherein the contact angle of a water drop on the non-stick layer of the metal cooking pot is θ, wherein 125°≤θ≤126°.
[0034] By adopting the above technical solution, the beneficial effects of the present invention are:
[0035] The present invention constructs an integrated micro-nano hydrophobic structure on the surface of the aluminum alloy pot embryo. After removing the oxide film and etching to form micron pits, a loose AlOOH film layer is formed by constant current anodizing. AlOOH-SiO2 composite sol is further sprayed on the surface of the loose AlOOH film layer. After that, the loose AlOOH film layer and the AlOOH-SiO2 particles on the surface and in the gaps of the loose AlOOH film layer are simultaneously converted into Al2O3-SiO2 particles on the surface and in the gaps of the loose Al2O3 film layer in combination with heating. Since the loose Al2O3 film layer is directly formed on the aluminum alloy pot embryo, the Al2O3 film layer is directly formed on the aluminum alloy pot embryo. The Al2O3 loose Al2O3 film layer on the surface of the alloy pot embryo and the Al2O3-SiO2 particles are synchronously transformed, and the lattice has a continuous structure, thus forming a micro-nano hydrophobic structure with a continuous structure from the aluminum alloy pot embryo-loose Al2O3 film layer-Al2O3-SiO2 particles; the formation process of the Al2O3-SiO2 particles is as follows: cross-linking in the composite gel to form Al-O-Si bonds, so as the SiO2 particles along the thickness direction of the pot embryo also grow together with the Al2O3 in the loose Al2O3 film layer, the non-stick layer obtained by the present invention has a stable structure;
[0036] The non-stick property of the present invention is formed by orderly arrangement of inorganic materials, the contact angle of the inorganic non-stick layer with water is between 125° and 126°, and the inorganic non-stick layer is integrally connected with the aluminum alloy pan body, so the non-stick effect is stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The present invention relates to a process flow chart for preparing a metal cooking pot;
[0038] Figure 2 yes Figure 1 Enlarged view of point A in the middle;
[0039] Figure 3 This is a photo of the contact angle of the metal cooking pot before friction in the comparative example;
[0040] Figure 4 This is a photo of the contact angle of the metal cooking pot after friction in the comparative example;
[0041] Figure 5 is a photograph of the contact angle of the metal cooking pot before friction in Example 1;
[0042] Figure 6 This is a photo of the contact angle of the metal cooking pot after friction in Example 1. DETAILED DESCRIPTION
[0043] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.
[0044] Example 1
[0045] This embodiment discloses a method for preparing a non-stick layer of a metal cooking pot. The specific preparation process is as follows: Figure 1 As shown, the following steps are included:
[0046] S1. Shot peening the aluminum alloy pot embryo to remove the surface oxide film, cleaning and drying;
[0047] S2, spraying acid solution onto the surface of the pot embryo to etch and form a micron pit structure;
[0048] The acid solution for etching in S2 is a mixture of H2SO4 and HF, and its composition is as follows:
[0049] The concentration of H2SO4 is 0.5 mol / L;
[0050] The HF concentration is 0.002 mol / L.
[0051] S3, subjecting the pot embryo body having a micron concave-convex structure obtained by surface etching to constant current anodizing;
[0052] The constant current anodization in S3 includes a start-up phase of 0V to 100V, a rising phase of voltage from 100V to 120V, and a constant voltage phase of 140V to 160V, and a loose AlOOH film layer is formed on the surface;
[0053] Constant current anodization is 30mA / cm 2 ;
[0054] The electrolyte is an aqueous solution of 0.2 mol / L oxalic acid;
[0055] The temperature of anodizing is 6°C;
[0056] The anodizing time was 3000 s.
[0057] S4, coating the surface of the loose AlOOH film layer with AlOOH-SiO2 composite sol, spraying it on the loose AlOOH film layer obtained in S3, drying it, and baking it;
[0058] The viscosity of AlOOH-SiO2 composite sol is 500mPa·s.
[0059] The spraying process of S4 is as follows:
[0060] AlOOH-SiO2 composite sol liquid is sprayed on the loose AlOOH film layer, and the spraying amount of AlOOH-SiO2 composite sol is 80g / m 2 .
[0061] S5. Heating. The AlOOH-SiO2 composite sol grows on the surface of the loose AlOOH film layer and in the gaps to become particles attached to the surface of the loose AlOOH film layer and in the gaps. The AlOOH-SiO2 particles and the AlOOH in the loose AlOOH film layer simultaneously lose water and are converted into Al2O3 during the heating process.
[0062] The process conditions for heating in S5 are as follows:
[0063] The temperature is 500°C and the time is 2 hours.
[0064] The preparation method of the AlOOH-SiO2 composite sol in S5 in this embodiment is as follows:
[0065] The separately prepared AlOOH sol and SiO2 sol were mixed in a molar ratio of Al to Si of 2.2:1;
[0066] After aging at room temperature for 24 hours, AlOOH-SiO2 composite sol was obtained.
[0067] The preparation method of AlOOH-SiO2 composite sol in this embodiment comprises the following steps:
[0068] S11, mixing Al(OC3H7)3 with deionized water for hydrolysis, then adding HNO3 and stirring in a water bath to obtain AlOOH sol;
[0069] The molar ratio of Al(OC3H7)3, deionized water and HNO3 is 1:150:0.3;
[0070] S12, adding tetraethyl orthosilicate and ethanol solution to the AlOOH sol obtained in S11, adding HNO3 to adjust the pH value to 3.1, and stirring to obtain a transparent and stable sol;
[0071] The molar ratio of ethyl orthosilicate to ethanol in S12 is 1:18.
[0072] The structure of the non-stick layer made on the aluminum alloy pan body in this embodiment is as follows Figure 2 As shown, it includes a pot body 100 and a non-stick layer 200 integrally connected to the pot body 100, wherein the non-stick layer 200 includes, in a direction away from the pot body 100, a loose Al2O3 film layer 201 grown on the pot body 100 and Al2O3-SiO2 particles 202 dispersed on the surface and in the gaps of the loose Al2O3 film layer 201, and the loose Al2O3 film layer 201 and the Al2O3-SiO2 particles 202 are connected through the continuously grown Al2O3 to form the non-stick layer 200 with a micro-nano hydrophobic structure.
[0073] Example 2
[0074] This embodiment discloses a method for preparing a non-stick layer of a metal cooking pot, comprising the following steps:
[0075] S1. Shot peening the aluminum alloy pot embryo to remove the surface oxide film, cleaning and drying;
[0076] S2, spraying acid solution onto the surface of the pot embryo to etch and form a micron pit structure;
[0077] The acid solution for etching in S2 is a mixture of H2SO4 and HF, and its composition is as follows:
[0078] The concentration of H2SO4 is 0.6 mol / L;
[0079] The HF concentration is 0.005 mol / L.
[0080] S3, subjecting the pot embryo body having a micron concave-convex structure obtained by surface etching to constant current anodizing;
[0081] The constant current anodization in S3 includes a start-up phase of 0V to 100V, a rising phase of voltage from 100V to 120V, and a constant voltage phase of 140V to 160V, and a loose AlOOH film layer is formed on the surface;
[0082] Constant current anodization is 30mA / cm 2 ;
[0083] The electrolyte is an aqueous solution of 0.2 mol / L oxalic acid;
[0084] The temperature of anodizing is 7°C;
[0085] The anodizing time was 3000 s.
[0086] S4, coating the surface of the loose AlOOH film layer with AlOOH-SiO2 composite sol, spraying it on the loose AlOOH film layer obtained in S3, drying it, and baking it;
[0087] The viscosity of AlOOH-SiO2 composite sol is 700mPa·s.
[0088] The spraying process of S4 is as follows:
[0089] The AlOOH-SiO2 composite sol is sprayed on the loose AlOOH film layer in liquid form. The spraying amount of the AlOOH-SiO2 composite sol is 100g / m 2 .
[0090] S5. Heating. The AlOOH-SiO2 composite sol grows on the surface of the loose AlOOH film layer and in the gaps to become particles attached to the surface of the loose AlOOH film layer and in the gaps. The AlOOH-SiO2 particles and the AlOOH in the loose AlOOH film layer simultaneously lose water and are converted into Al2O3 during the heating process.
[0091] The process conditions for heating in S5 are as follows:
[0092] The temperature is 600°C and the time is 2 hours.
[0093] The preparation method of the AlOOH-SiO2 composite sol in S5 in this embodiment is as follows:
[0094] The separately prepared AlOOH sol and SiO2 sol were mixed in a molar ratio of Al to Si of 2.5:1;
[0095] After aging at room temperature for 24 hours, AlOOH-SiO2 composite sol was obtained.
[0096] The preparation method of AlOOH-SiO2 composite sol in this embodiment comprises the following steps:
[0097] S11, mixing Al(OC3H7)3 with deionized water for hydrolysis, then adding HNO3 and stirring in a water bath to obtain AlOOH sol;
[0098] The molar ratio of Al(OC3H7)3, deionized water and HNO3 is 1:160:0.4;
[0099] S12, adding ethyl orthosilicate and ethanol solution to the AlOOH sol obtained in S11, adding HNO3 to adjust the pH value to 3.5, and stirring to obtain a transparent and stable sol;
[0100] The molar ratio of ethyl orthosilicate to ethanol in S12 is 1:19.
[0101] Example 3
[0102] This embodiment discloses a method for preparing a non-stick layer of a metal cooking pot, comprising the following steps:
[0103] S1. Shot peening the aluminum alloy pot embryo to remove the surface oxide film, cleaning and drying;
[0104] S2, spraying acid solution onto the surface of the pot embryo to etch and form a micron pit structure;
[0105] The acid solution for etching in S2 is a mixture of H2SO4 and HF, and its composition is as follows:
[0106] The concentration of H2SO4 is 0.6 mol / L;
[0107] The HF concentration is 0.002 mol / L.
[0108] S3, subjecting the pot embryo body having a micron concave-convex structure obtained by surface etching to constant current anodizing;
[0109] The constant current anodization in S3 includes a start-up phase of 0V to 100V, a rising phase of voltage from 100V to 120V, and a constant voltage phase of 140V to 160V, and a loose AlOOH film layer is formed on the surface;
[0110] Constant current anodization is 30mA / cm 2 ;
[0111] The electrolyte is an aqueous solution of 0.2 mol / L oxalic acid;
[0112] The temperature of anodizing is 8°C;
[0113] The anodizing time was 3000 s.
[0114] S4, coating the surface of the loose AlOOH film layer with AlOOH-SiO2 composite sol, spraying it on the loose AlOOH film layer obtained in S3, drying it, and baking it;
[0115] The viscosity of AlOOH-SiO2 composite sol is 1000 mPa·s.
[0116] The spraying process of S4 is as follows:
[0117] AlOOH-SiO2 composite sol liquid is sprayed on the loose AlOOH film layer, and the spraying amount of AlOOH-SiO2 composite sol is 120g / m 2 .
[0118] S5. Heating. The AlOOH-SiO2 composite sol grows on the surface of the loose AlOOH film layer and in the gaps to become particles attached to the surface of the loose AlOOH film layer and in the gaps. The AlOOH-SiO2 particles and the AlOOH in the loose AlOOH film layer simultaneously lose water and are converted into Al2O3 during the heating process.
[0119] The process conditions for heating in S5 are as follows:
[0120] The temperature is 550°C and the time is 3 hours. The preparation method of the AlOOH-SiO2 composite sol in S5 in this embodiment is as follows:
[0121] The separately prepared AlOOH sol and SiO2 sol were mixed in a molar ratio of Al to Si of 2.8:1;
[0122] After aging at room temperature for 24 hours, AlOOH-SiO2 composite sol was obtained.
[0123] The preparation method of AlOOH-SiO2 composite sol in this embodiment comprises the following steps:
[0124] S11, mixing Al(OC3H7)3 with deionized water for hydrolysis, then adding HNO3 and stirring in a water bath to obtain AlOOH sol;
[0125] The molar ratio of Al(OC3H7)3, deionized water and HNO3 is 1:170:0.5;
[0126] S12, adding ethyl orthosilicate and ethanol solution to the AlOOH sol obtained in S11, adding HNO3 to adjust the pH value to 3.7, and stirring to obtain a transparent and stable sol;
[0127] The molar ratio of ethyl orthosilicate to ethanol in S12 is 1:20.
[0128] Example 4
[0129] This embodiment discloses a method for preparing a non-stick layer of a metal cooking pot, comprising the following steps:
[0130] S1. Shot peening the aluminum alloy pot embryo to remove the surface oxide film, cleaning and drying;
[0131] S2, spraying acid solution onto the surface of the pot embryo to etch and form a micron pit structure;
[0132] The acid solution for etching in S2 is a mixture of H2SO4 and HF, and its composition is as follows:
[0133] The concentration of H2SO4 is 0.5 mol / L;
[0134] The HF concentration is 0.005 mol / L.
[0135] S3, subjecting the pot embryo body having a micron concave-convex structure obtained by surface etching to constant current anodizing;
[0136] The constant current anodization in S3 includes a start-up phase of 0V to 100V, a rising phase of voltage from 100V to 120V, and a constant voltage phase of 140V to 160V, and a loose AlOOH film layer is formed on the surface;
[0137] Constant current anodization is 30mA / cm 2 ;
[0138] The electrolyte is an aqueous solution of 0.2 mol / L oxalic acid;
[0139] The temperature of anodizing is 7°C;
[0140] The anodizing time was 3000 s.
[0141] S4, coating the surface of the loose AlOOH film layer with AlOOH-SiO2 composite sol, spraying it on the loose AlOOH film layer obtained in S3, drying it, and baking it;
[0142] The viscosity of AlOOH-SiO2 composite sol is 600mPa·s.
[0143] The spraying process of S4 is as follows:
[0144] AlOOH-SiO2 composite sol liquid is sprayed on the loose AlOOH film layer, and the spraying amount of AlOOH-SiO2 composite sol is 90g / m 2 .
[0145] S5. Heating. The AlOOH-SiO2 composite sol grows on the surface of the loose AlOOH film layer and in the gaps to become particles attached to the surface of the loose AlOOH film layer and in the gaps. The AlOOH-SiO2 particles and the AlOOH in the loose AlOOH film layer simultaneously lose water and are converted into Al2O3 during the heating process.
[0146] The process conditions for heating in S5 are as follows:
[0147] The temperature is 600°C and the time is 3 hours.
[0148] The preparation method of the AlOOH-SiO2 composite sol in S5 in this embodiment is as follows:
[0149] The separately prepared AlOOH sol and SiO2 sol were mixed in a molar ratio of Al to Si of 3.3:1;
[0150] After aging at room temperature for 24 hours, AlOOH-SiO2 composite sol was obtained.
[0151] The preparation method of AlOOH-SiO2 composite sol in this embodiment comprises the following steps:
[0152] S11, mixing Al(OC3H7)3 with deionized water for hydrolysis, then adding HNO3 and stirring in a water bath to obtain AlOOH sol;
[0153] The molar ratio of Al(OC3H7)3, deionized water and HNO3 is 1:180:0.6;
[0154] S12, adding ethyl orthosilicate and ethanol solution to the AlOOH sol obtained in S11, adding HNO3 to adjust the pH value to 3.8, and stirring to obtain a transparent and stable sol;
[0155] The molar ratio of ethyl orthosilicate to ethanol in S12 is 1:18.
[0156] Example 5
[0157] This embodiment discloses a method for preparing a non-stick layer of a metal cooking pot, comprising the following steps:
[0158] S1. Shot peening the aluminum alloy pot embryo to remove the surface oxide film, cleaning and drying;
[0159] S2, spraying acid solution onto the surface of the pot embryo to etch and form a micron pit structure;
[0160] The acid solution for etching in S2 is a mixture of H2SO4 and HF, and its composition is as follows:
[0161] The concentration of H2SO4 is 0.5 mol / L;
[0162] The HF concentration is 0.003 mol / L.
[0163] S3, subjecting the pot embryo body having a micron concave-convex structure obtained by surface etching to constant current anodizing;
[0164] The constant current anodization in S3 includes a start-up phase of 0V to 100V, a rising phase of voltage from 100V to 120V, and a constant voltage phase of 140V to 160V, and a loose AlOOH film layer is formed on the surface;
[0165] Constant current anodization is 30mA / cm 2 ;
[0166] The electrolyte is an aqueous solution of 0.2 mol / L oxalic acid;
[0167] The temperature of anodizing is 6°C;
[0168] The anodizing time was 3000 s.
[0169] S4, coating the surface of the loose AlOOH film layer with AlOOH-SiO2 composite sol, spraying it on the loose AlOOH film layer obtained in S3, drying it, and baking it;
[0170] The viscosity of AlOOH-SiO2 composite sol is 800mPa·s.
[0171] The spraying process of S4 is as follows:
[0172] The AlOOH-SiO2 composite sol is sprayed on the loose AlOOH film layer in liquid form. The spraying amount of the AlOOH-SiO2 composite sol is 100g / m 2 .
[0173] S5. Heating. The AlOOH-SiO2 composite sol grows on the surface of the loose AlOOH film layer and in the gaps to become particles attached to the surface of the loose AlOOH film layer and in the gaps. The AlOOH-SiO2 particles and the AlOOH in the loose AlOOH film layer simultaneously lose water and are converted into Al2O3 during the heating process.
[0174] The process conditions for heating in S5 are as follows:
[0175] The temperature is 550°C and the time is 2 hours.
[0176] The preparation method of the AlOOH-SiO2 composite sol in S5 in this embodiment is as follows:
[0177] The separately prepared AlOOH sol and SiO2 sol were mixed in a molar ratio of Al to Si of 3.1:1;
[0178] After aging at room temperature for 24 hours, AlOOH-SiO2 composite sol was obtained.
[0179] The preparation method of AlOOH-SiO2 composite sol in this embodiment comprises the following steps:
[0180] S11, mixing Al(OC3H7)3 with deionized water for hydrolysis, then adding HNO3 and stirring in a water bath to obtain AlOOH sol;
[0181] The molar ratio of Al(OC3H7)3, deionized water and HNO3 is 1:180:0.3;
[0182] S12, adding ethyl orthosilicate and ethanol solution to the AlOOH sol obtained in S11, adding HNO3 to adjust the pH value to 3.9, and stirring to obtain a transparent and stable sol;
[0183] The molar ratio of ethyl orthosilicate to ethanol in S12 is 1:19.
[0184] Comparative Example
[0185] In this example, the method for preparing a non-stick layer on an aluminum alloy pan body used in Examples 1 to 5 includes the following steps:
[0186] S1. Shot peening the aluminum alloy pot embryo to remove the surface oxide film, cleaning and drying;
[0187] S2, spraying acid solution onto the surface of the pot embryo to etch and form a micron pit structure;
[0188] The acid solution for etching in S2 is a mixture of H2SO4 and HF, and its composition is as follows:
[0189] The concentration of H2SO4 is 0.5 mol / L;
[0190] HF concentration is 0.002 mol / L;
[0191] S3. Spray Teflon coating onto the pot embryo body after S2, with the coating thickness of 28 μm.
[0192] In order to facilitate the test of contact angle, a non-stick layer was prepared on the surface of the aluminum alloy with sheet structure prepared in Examples 1 to 5 and the comparative example, and the wear resistance of the obtained non-stick layer and the change of contact angle before and after wear at 230°C were tested.
[0193] Fix the cleaned and dried pots and steel wool on the testing machine in a greenhouse, apply a force of 1.5 kg on the connecting rod that fixes the steel wool, adjust the frequency to 60 times / min and the back and forth movement distance to 100 mm, start the testing machine, and record the number of cycles; replace the steel wool every 10,000 times. After the number of cycles is completed, test the non-stickiness. The non-stickiness test method refers to GB / T32388-2015.
[0194] Table 1 Wear resistance cycle number of the non-stick layer on the aluminum alloy surface obtained in Examples 1 to 5 and Comparative Examples
[0195] project Cycle times Example 1 85,000 times Example 2 88,000 times Example 3 90,000 times Example 4 85,000 times Example 5 88,000 times Comparative Example 10,000 times
[0196] The wear resistance of the non-stick layer obtained in Examples 1 to 5 is significantly improved compared with that of the non-stick layer obtained in the comparative example. It can be seen that the loose AlOOH film layer is integrally formed on the surface of the aluminum alloy pot embryo by constant current anodizing, and AlOOH-SiO2 composite sol is further sprayed on the surface of the loose AlOOH film layer, and then the loose AlOOH film layer and the AlOOH-SiO2 particles on its surface and in the gaps are synchronously converted into loose Al2O3 film layer and Al2O3-SiO2 particles on its surface and in the gaps in combination with heating. Since the loose Al2O3 film layer is directly connected to the surface of the aluminum alloy pot embryo, and the Al2O3 in the Al2O3-SiO2 particles is The lattice of the aluminum alloy pot embryo is synchronously transformed, and has a continuous structure. Thus, a micro-nano hydrophobic structure with continuous Al2O3 connection is formed from the aluminum alloy pot embryo - loose Al2O3 film layer - Al2O3 - SiO2 particles. Therefore, when the non-stick layer is subjected to external force, the force can be dispersed due to the continuous connection structure between the non-stick layer and the aluminum alloy pot embryo, and its wear resistance is significantly improved. At this time, the Teflon coating and the aluminum alloy pot embryo in the comparative example are still an interlayer bonding structure. When subjected to external force, the two are easily separated at the interface due to the inconsistent deformation, and then fall off and separate under the action of further external force. Therefore, the wear resistance of the non-stick layer integrally connected with the aluminum alloy pot embryo obtained in the present invention is significantly improved.
[0197] The formation process of Al2O3-SiO2 particles that form a micro-nano hydrophobic structure is as follows: cross-linking in the composite gel to form Al-O-Si bonds, so that along the thickness direction of the pot embryo, the SiO2 particles also grow together with Al2O3 in the loose Al2O3 film layer; the sol forms AlOOH particles during the drying and heating process, which are further converted into Al2O3, and Al2O3 grows in the aluminum alloy pot embryo. Al2O3-SiO2 particles continuously grow from the loose Al2O3 film layer, and an inorganic non-stick layer is formed by the orderly arrangement of inorganic materials, as shown in Table 2. The contact angle of the inorganic non-stick layer obtained by the present invention has a stable structure at a higher use temperature, resulting in strong wear resistance at high temperatures. Further simulate the friction of the non-stick layer in the use state, and test the change in the contact angle of water of the non-stick layer before and after 3000 frictions under 230°C. The specific test method is as follows:
[0198] Fix the cleaned and dried pot and steel wool on the testing machine, heat the pot to 230°C, apply a force of 1.5 kg on the connecting rod that fixes the steel wool, adjust the frequency to 60 times / min and the reciprocating distance to 100 mm, and start the testing machine; the specific test data are shown in Table 2.
[0199] Table 2 Changes in contact angle of the non-stick layer obtained in Examples 1 to 5 and Comparative Examples before and after high temperature friction
[0200] project Contact angle before friction Contact angle after friction Contact angle change Example 1 126.0° 122.3° -3.7° Example 2 124.3° 120.3° -4.0° Example 3 123.3° 117.9° -5.4° Example 4 125.8° 118.5° -7.3° Example 5 125.0° 119.8° -5.2° Comparative Example 118.5° 96.5° -22.0°
[0201] The contact angle test pictures of the comparative example and embodiment 2 are as follows: Figures 3 to 6 shown.
[0202] From Table 2, it can be seen that the inorganic non-stick film layer obtained in the present invention has a hydrophobic micro-nano structure, and the non-stick layer is connected to the aluminum alloy pot body structure as an integrated structure. After rubbing 3000 times at a temperature of 230°C, the non-stick loss is small, which proves that the non-stick layer structure changes little and the non-stick layer structure is stable.
Claims
1. A method for preparing a non-stick layer of a metal cooking pot, Features: The following steps are involved: S1. Shot peening the aluminum alloy pot embryo to remove the surface oxide film, cleaning and drying; S2, spraying acid solution onto the surface of the pot embryo to etch and form a micron pit structure; S3, subjecting the pot embryo body having a micron concave-convex structure obtained by surface etching to constant current anodizing; S4, AlOOH-SiO is coated on the surface of the loose AlOOH film layer. 2 The composite sol is sprayed on the loose AlOOH film obtained by S3, dried, and baked; S5, heating, AlOOH-SiO 2 The composite sol grows on the surface and in the gaps of the loose AlOOH film layer to form particles attached to the surface and in the gaps of the loose AlOOH film layer. 2 The AlOOH in the granular and loose AlOOH film is converted into Al simultaneously during heating. 2 O 3 .
2. The preparation method according to claim 1, Features: The etching acid in S2 is H 2 SO 4 The mixture of HF and MgSO4 has the following composition: H 2 SO 4 The concentration is 0.5 to 0.6 mol / L; The HF concentration is 0.002 to 0.005 mol / L.
3. The preparation method according to claim 1, Features: The constant current anodization in S3 includes a start-up phase of 0V to 100V, a rising phase of voltage from 100V to 120V, and a constant voltage phase of 140V to 160V, and a loose AlOOH film layer is formed on the surface; Constant current anodization is 30mA / cm 2 ; The electrolyte is an aqueous solution of 0.2 mol / L oxalic acid; The temperature of anodization is 6°C to 8°C.
4. The preparation method according to claim 1, Features: AlOOH-SiO 2 The viscosity of the composite sol is 500 mPa·s to 1000 mPa·s.
5. The preparation method according to claim 1, Features: The spraying process of S4 is as follows: AlOOH-SiO 2 The composite sol liquid is sprayed on the loose AlOOH film layer; AlOOH-SiO 2 The spraying amount of composite sol is 80g / m 2 Up to 120g / m 2 .
6. The preparation method according to claim 1, Features: The process conditions for heating in S5 are as follows: The temperature is 500°C to 600°C; the time is 2 hours to 3 hours.
7. The preparation method according to claim 1, Features: AlOOH-SiO in S5 2 The preparation method of the composite sol is as follows: The prepared AlOOH sol and SiO 2 The sol was mixed in a molar ratio of Al to Si of (2.1 to 3.3):1; After aging at room temperature for 24 hours, AlOOH-SiO 2 Composite sol.
8. The preparation method according to claim 7, It is characterized in that: It is characterized in that: AlOOH-SiO 2 The preparation method of the composite sol comprises the following steps: S11, Al(OC 3 H 7 ) 3 Mix with deionized water for hydrolysis, then add HNO 3 , stirring in a water bath to obtain AlOOH sol; Among them, Al(OC 3 H 7 ) 3 , deionized water and HNO 3 The molar ratio is 1:(150 to 180):(0.3 to 0.6); S12, add ethyl orthosilicate and ethanol solution to the AlOOH sol obtained in S11, add HNO 3 Adjust the pH value to 3 to 4 and stir to obtain a transparent and stable sol; The molar ratio of ethyl orthosilicate to ethanol in S12 is 1:(18 to 20).