Method for producing cobalt sulfate

By implementing solvent extraction, copper removal and carboxylic acid extraction processes in the cobalt chloride solution, combined with the adjustment of pH value and redox potential, impurities were successfully removed from the cobalt chloride solution, and high-purity cobalt sulfate solution and The crystal solves the problem of high manufacturing cost in the existing technology and realizes efficient cobalt sulfate manufacturing.

CN116056774BActive Publication Date: 2024-10-01SUMITOMO METAL MINING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280006328.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-11
Filing Date
2022-01-06
Publication Date
2024-10-01
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

The existing technology requires an electrolysis process or a method that increases the cost of processes and chemicals when manufacturing high-purity cobalt sulfate, resulting in high manufacturing costs and difficulty in obtaining cobalt sulfate solution directly from cobalt chloride solution.

Method used

The solvent extraction process, copper removal process and second solvent extraction process are implemented in sequence, using alkyl phosphoric acid series and carboxylic acid series extractants to remove impurity elements respectively, and by adjusting the pH value and redox potential, the separation and reversal of cobalt are achieved. Extraction is performed to obtain a high-purity cobalt sulfate solution, and crystallization is performed to obtain cobalt sulfate crystals without using an electrolysis process.

Benefits of technology

Without increasing the cost of processes and chemicals, the impurities were successfully removed from the impurity-containing cobalt chloride solution, a high-purity cobalt sulfate solution was directly produced, and high-purity cobalt sulfate crystals were obtained through crystallization, reducing manufacturing costs. , improving process efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116056774B_ABST
    Figure CN116056774B_ABST
Patent Text Reader

Abstract

A method for producing cobalt sulfate is provided, wherein impurities and cobalt are separated from a cobalt chloride solution containing impurities without using an electrolysis process, thereby producing cobalt sulfate with high purity. The following processes are sequentially performed: a first solvent extraction process (S1), wherein the cobalt chloride solution containing impurities is contacted with an organic solvent containing an alkylphosphoric acid-based extractant, zinc, manganese and calcium are extracted into the organic solvent and separated and removed; a copper removal process (S2), wherein a sulfiding agent is added to the cobalt chloride solution, copper sulfide precipitation is generated and separated and removed; a second solvent extraction process (S3), wherein the cobalt chloride solution is contacted with an organic solvent containing a carboxylic acid extractant, cobalt is extracted into the organic solvent, and then cobalt is reversely extracted with sulfuric acid to obtain a cobalt sulfate solution; and a crystallization process (S4), which is performed on the cobalt sulfate solution obtained through the second solvent extraction process (S3). Impurities including magnesium can be separated from cobalt without using an electrolysis process, thereby directly producing high-purity cobalt sulfate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing cobalt sulfate, and more particularly to a method for producing cobalt sulfate with high purity by removing impurity elements contained in a cobalt chloride solution. Background Art

[0002] Cobalt is a valuable metal that is widely used in industrial applications as a raw material for magnetic materials or lithium-ion batteries, in addition to being used as an additive element for special alloys. In particular, recently, lithium-ion secondary batteries have been used more and more as batteries for mobile devices or electric vehicles, and the demand for cobalt has also expanded rapidly. However, most cobalt is produced as a by-product of nickel or copper smelting, so separating it from impurities represented by nickel or copper has become an important key technology in the manufacture of cobalt.

[0003] For example, when cobalt is recovered as a by-product in the wet smelting of nickel, first, in order to obtain a solution containing nickel and cobalt, the raw material is leached or extracted into a solution or the raw material is dissolved using a mineral acid or an oxidant. Furthermore, the nickel and cobalt contained in the obtained acidic solution are often separated and recovered by a solvent extraction method using various organic extractants according to a previously known method.

[0004] However, the obtained cobalt solution often contains various impurities from the processed raw materials.

[0005] Therefore, it is necessary to further remove impurity elements such as manganese, copper, zinc, calcium and magnesium from the cobalt solution after nickel is separated and recovered by the above-mentioned solvent extraction method.

[0006] Furthermore, in order to produce high-purity cobalt products with a low impurity content, it is necessary to remove impurity elements from a cobalt solution separated and recovered from a nickel solution containing cobalt in advance, and then convert it into a cobalt product through an electrolysis process or crystallization.

[0007] As a method for removing impurity elements in a cobalt solution, there are conventional technologies described in Patent Documents 1 and 2.

[0008] Patent Document 1 discloses a method for purifying a cobalt solution, which comprises: (1) a copper removal step, in which a sulfiding agent is added to the cobalt solution to adjust the oxidation-reduction potential (ORP) (Ag / AgCl electrode basis) to 50 mV or less and the pH value is adjusted to 0.3 to 2.4, thereby obtaining a copper sulfide precipitate and a copper-desulfurized purified solution; (2) a manganese removal step, in which an oxidizing agent and a neutralizing agent are added to the copper-desulfurized purified solution to adjust the oxidation-reduction potential (Ag / AgCl electrode basis) to 950 to 1050 mV and the pH value to 2.4 to 3.0, thereby obtaining a manganese precipitate and a manganese-desulfurized purified solution; and (3) a solvent extraction step, in which an alkylphosphoric acid is used as an extractant in the manganese-desulfurized purified solution to extract and separate zinc, calcium and trace impurities in the manganese-desulfurized purified solution.

[0009] Patent document 2 describes a separation technology, which is to contact a cobalt chloride solution having a hydrochloric acid concentration of 2 to 6 mol / L with an anion exchange resin, so that metal impurities such as iron, zinc, and tin are adsorbed and separated by forming a complex having a distribution coefficient with respect to the anion exchange resin greater than the distribution coefficient of the cobalt chloride complex with respect to the anion exchange resin.

[0010] The solvent extraction method using alkylphosphoric acid as an extractant described in Patent Document 1 has high separation performance for zinc or calcium. However, in the case of a cobalt chloride solution having a hydrochloric acid concentration of 2 to 6 mol / L, an ion exchange method using an anion exchange resin or a solvent extraction method using an amine-based extractant has higher separation performance for zinc and cobalt than the solvent extraction method using alkylphosphoric acid.

[0011] In addition, when removing a very small amount of zinc in a cobalt chloride solution, the ion exchange method is more efficient and economical because the process and operation are simple.

[0012] From this viewpoint, as a method for removing these impurity elements from a cobalt chloride solution containing manganese, copper, and zinc, a method combining the purification method of Patent Document 1 and the separation technology of Patent Document 2 has been proposed (for example, Patent Document 3).

[0013] The method for producing high-purity cobalt chloride described in paragraph 0022 of Patent Document 3 includes a solvent extraction step for separating nickel and cobalt, a manganese removal step for removing manganese, a copper removal step for removing copper, a zinc removal step for removing zinc, and an electrolysis step.

[0014] In the dezincification process, the aqueous cobalt chloride solution obtained in the decopperization process is brought into contact with an anion exchange resin to remove zinc by adsorption. In the electrolysis process, the high-purity aqueous cobalt chloride solution obtained in the dezincification process is used as an electrolysis feed solution to produce metallic cobalt (also called electric cobalt).

[0015] On the other hand, as described above, the demand for cobalt as a raw material for lithium ion secondary batteries has recently expanded, and the form of a cobalt sulfate solution or cobalt sulfate crystals is desired.

[0016] If one wants to obtain cobalt sulfate crystals from the metal cobalt obtained by the prior art of Patent Document 3, the metal cobalt is dissolved in sulfuric acid to obtain a cobalt sulfate solution, and then the solution is crystallized to obtain cobalt sulfate crystals. However, if this manufacturing method is used, the manufacturing cost is increased due to the increase in steps or the increase in reagent costs. In addition, the dissolution rate of plate-shaped metal cobalt in sulfuric acid is relatively slow, as is the case for corrosion-resistant alloys. In order to dissolve it in a short time, the plate-shaped metal cobalt needs to be powdered by atomization or the like.

[0017] Therefore, a method for obtaining a cobalt sulfate solution directly from a cobalt chloride solution without going through metallic cobalt is desired.

[0018] Prior art literature

[0019] Patent Literature

[0020] Patent Document 1: Japanese Patent Application Publication No. 2004-285368.

[0021] Patent document 2: Japanese Patent Application Publication No. 2001-020021.

[0022] Patent document 3: Japanese Patent Application Publication No. 2020-19664. Summary of the invention

[0023] [Problems to be Solved by the Invention]

[0024] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing cobalt sulfate, which separates impurities from cobalt from a cobalt chloride solution containing impurities without using an electrolysis step to produce cobalt sulfate with high purity.

[0025] [Methods for solving the problem]

[0026] The method for producing cobalt sulfate of the first invention is characterized in that the following steps are carried out in order: a first solvent extraction step, in which a cobalt chloride solution containing one or more impurities of copper, zinc, manganese, calcium and magnesium is brought into contact with an organic solvent containing an alkylphosphoric acid-based extractant, zinc, manganese and calcium are extracted into the organic solvent and separated and removed; a copper removal step, in which a sulfiding agent is added to the cobalt chloride solution that has undergone the first solvent extraction step to generate a precipitate of copper sulfide and separate and remove it; and a second solvent extraction step, in which the cobalt chloride solution that has undergone the copper removal step is brought into contact with an organic solvent containing a carboxylic acid extractant, cobalt is extracted into the organic solvent, and then cobalt is reversely extracted with sulfuric acid to obtain a cobalt sulfate solution.

[0027] The method for producing cobalt sulfate of the second invention is characterized in that, in the first invention, in the above-mentioned first solvent extraction step, the alkylphosphoric acid-based extractant is bis(2-ethylhexyl) hydrogen phosphate, the pH value of the cobalt chloride solution is adjusted to 1.5 to 3.0, and solvent extraction using the above-mentioned extractant is carried out to extract the impurity elements into the organic solvent.

[0028] The method for producing cobalt sulfate of the third invention is characterized in that, in the first or second invention, in the above-mentioned copper removal step, an oxidizing agent and a neutralizing agent are added to a cobalt chloride solution to which a sulfiding agent is added, and the redox potential is adjusted to -100 to 200 mV based on an Ag / AgCl electrode, and the pH value is adjusted to 1.3 to 3.0.

[0029] The method for producing cobalt sulfate of the fourth invention is characterized in that, in the first, second or third invention, in the second solvent extraction step, an alkaline solution is added to the cobalt chloride solution from which copper, zinc, manganese and calcium have been removed, the pH value is adjusted to 5.0 to 7.0, and a cobalt extraction step of extracting cobalt into an organic solvent using a carboxylic acid-based extractant is carried out.

[0030] The method for producing cobalt sulfate of the fifth invention is characterized in that, in the first, second or third invention, after the above-mentioned cobalt extraction step in the above-mentioned second solvent extraction step, a sulfuric acid solution is brought into contact with an organic solvent in which cobalt is extracted, the pH value is adjusted to 2.0 to 4.5, and a cobalt reverse extraction step of reversely extracting cobalt into the sulfuric acid solution is carried out.

[0031] The method for producing cobalt sulfate according to the sixth invention is characterized in that, in the first invention, the cobalt sulfate solution obtained through the second solvent extraction step is subjected to a crystallization step to obtain cobalt sulfate crystals.

[0032] The method for producing cobalt sulfate of the seventh invention is characterized in that, in the first, second, third, fourth, fifth or sixth invention, the second solvent extraction step includes a solvent recovery treatment, which is the following treatment: the cobalt chloride solution after the cobalt is extracted is contacted with an organic solvent after the cobalt is back-extracted into a sulfuric acid solution, the pH value is adjusted to be greater than 2.0 and less than 4.0, and the carboxylic acid-based extractant in the cobalt chloride solution is separated.

[0033] [Effects of the Invention]

[0034] According to the first invention, a high-purity cobalt sulfate solution from which impurities have been removed can be obtained by performing a first solvent extraction step for separating and removing zinc, manganese and calcium, a copper removal step for precipitating copper in the form of sulfide, and a second solvent extraction step for separating and removing magnesium from a cobalt chloride solution containing impurities. Therefore, impurities can be separated from cobalt without using an electrolysis step, and high-purity cobalt sulfate can be directly produced.

[0035] According to the second invention, by adjusting the pH value to 1.5 to 3.0, cobalt can be left in the aqueous phase, and zinc, manganese and calcium can be extracted and separated from cobalt.

[0036] According to the third invention, copper sulfide can be precipitated from the cobalt chloride solution to be sufficiently removed, and coprecipitation of cobalt can be suppressed.

[0037] According to the fourth invention, cobalt can be extracted into the organic phase by adjusting the pH to 5.0 to 7.0 and contacting with an organic solvent containing a carboxylic acid-based extractant.

[0038] According to the fifth invention, the cobalt extracted into the organic phase can be brought into contact with a sulfuric acid solution and the pH value can be adjusted to 2.0 to 4.5, thereby back-extracting the cobalt into the sulfuric acid solution. In this way, a high-purity cobalt sulfate solution can be obtained.

[0039] According to the sixth invention, by further carrying out a crystallization step, high-purity cobalt sulfate crystals can be obtained from the cobalt sulfate solution.

[0040] According to the seventh invention, by performing the solvent recovery step of separating the carboxylic acid-based extractant in the cobalt chloride solution, it is possible to suppress the loss of the organic solvent contained in the cobalt chloride solution after extraction or suppress the increase in environmental load due to wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a process diagram showing the method for producing cobalt sulfate of the present invention.

[0042] Figure 2 This is a process diagram showing a method for producing cobalt sulfate according to one embodiment of the present invention.

[0043] Figure 3 yes Figure 2 Detailed process diagram of the first solvent extraction step S1 is shown.

[0044] Figure 4 yes Figure 2 Detailed process diagram of the second solvent extraction step S3 is shown.

[0045] Figure 5 It is a detailed process diagram of the solvent recovery process S32. DETAILED DESCRIPTION

[0046] Hereinafter, specific embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the gist of the present invention.

[0047] (Basic Principle of the Invention)

[0048] based on Figure 1The method for producing cobalt sulfate of the present invention will be described.

[0049] This production method is characterized by carrying out the following steps in order.

[0050] (1) A first solvent extraction step S1, in which a cobalt chloride solution containing one or more impurities of copper, zinc, manganese, calcium and magnesium is brought into contact with an organic solvent containing an alkylphosphoric acid-based extractant, and zinc, manganese and calcium are extracted into the organic solvent to be separated and removed.

[0051] (2) Copper removal step S2, in which a sulfidizing agent is added to the cobalt chloride solution from which zinc, manganese and calcium have been removed in the first solvent extraction step S1, to generate a precipitate of copper sulfide, which is then separated and removed.

[0052] (3) A second solvent extraction step S3, in which the cobalt chloride solution from which copper, zinc, manganese and calcium have been removed in the copper removal step S2 is contacted with an organic solvent containing a carboxylic acid extractant, cobalt is extracted into the organic solvent, and then the cobalt is reversely extracted with sulfuric acid to obtain a cobalt sulfate solution. In addition, the second solvent extraction step S3 preferably includes a solvent recovery process S32.

[0053] In the present invention, after each of the above steps S1 to S3, a crystallization step S4 of precipitating crystals from the cobalt sulfate solution is performed as necessary.

[0054] Furthermore, Figure 1 Although not shown in the figure, after the first solvent extraction step S1 and / or after the second solvent extraction step S3, a step of subjecting the liquid to an oil-water separation device such as an activated carbon column to separate and remove organic components mixed in the liquid may be added.

[0055] In the present invention, the cobalt chloride solution as the starting material contains one or more of copper, zinc, manganese, calcium and magnesium as impurity elements. As long as it is such a cobalt chloride solution containing impurities, it is not subject to any limitation on the application of the present invention, but is particularly suitable for the cobalt chloride solution after nickel is separated and recovered from the nickel solution containing cobalt by an alkylphosphoric acid-based extractant or an amine-based extractant in the solvent extraction process of nickel smelting.

[0056] According to the present invention, zinc, manganese and calcium can be separated and removed from a cobalt chloride solution containing impurities through the first solvent extraction step S1, copper can be removed by generating copper sulfide precipitation through the copper removal step S2, and magnesium can be separated and removed through the second solvent extraction step S3, thereby obtaining a high-purity cobalt sulfate solution. Therefore, impurities can be separated from cobalt without using an electrolysis step, and a high-purity cobalt sulfate solution can be directly manufactured. In addition, the carboxylic acid-based extractant can be separated and recovered through the solvent recovery process S32 included in the second solvent extraction step S3.

[0057] According to the present invention, by subjecting the cobalt sulfate solution after the above steps S1 to S3 to the crystallization step S4, crystals can be precipitated from the solution to obtain cobalt sulfate crystals.

[0058] (Implementation Method)

[0059] The following is based on Figure 2 to Figure 5 An embodiment of the method for producing cobalt sulfate will be described. Figure 2 The summary shows Figure 1 Details of steps S1 to S3 are shown.

[0060] (First solvent extraction step S1)

[0061] based on Figure 2 and Figure 3 , the first solvent extraction step S1 is described.

[0062] The first solvent extraction step S1 is a step of bringing a cobalt chloride solution containing one or more impurities of copper, zinc, manganese, calcium and magnesium as a starting material into contact with an organic solvent containing an alkylphosphoric acid-based extractant, extracting zinc, manganese and calcium into the organic solvent and separating and removing them. In addition, a portion of copper may be extracted and separated and removed.

[0063] As the organic solvent, a solvent obtained by diluting an alkyl phosphoric acid-based extractant with a diluent can be used. Examples of the alkyl phosphoric acid-based extractant include bis(2-ethylhexyl) hydrogen phosphate (trade name: D2EHPA), 2-ethylhexyl (2-ethylhexyl) phosphonate (trade name: PC-88A), and di(2,4,4-trimethylpentyl) phosphinic acid (trade name: CYANEX272). Among these, when separating zinc, manganese, and calcium from a cobalt chloride solution from which copper has been removed, it is more preferable to use bis(2-ethylhexyl) hydrogen phosphate as an extractant because it has a higher separation property from cobalt.

[0064] The diluent is not particularly limited as long as it can dissolve the extractant. As the diluent, for example, cycloalkane solvents and aromatic solvents can be used. The concentration of the extractant is preferably adjusted to 10 to 60% by volume, and more preferably adjusted to 20 to 50% by volume. If the concentration of the extractant is within this range, both the impurity elements with a higher concentration and the impurity elements with a lower distribution ratio (element concentration in the organic solvent / element concentration in the solution) can be fully extracted. On the other hand, when the concentration of the extractant is less than 10%, the impurity elements with a higher concentration or the impurity elements with a lower distribution ratio cannot be fully extracted and are likely to remain in the cobalt chloride solution. In addition, when the concentration of the extractant exceeds 60%, the viscosity of the organic solvent becomes higher, and the phase separation of the organic solvent (organic phase) and the cobalt chloride solution (aqueous phase) after the extraction operation will deteriorate.

[0065] As shown in Formula 4, an acidic extractant such as an alkylphosphoric acid-based extractant is an extractant that extracts metal ions by replacing -H possessed by the extractant with cations in the aqueous phase to form a metal salt. Generally speaking, if the pH value becomes higher, metal ions are easily extracted into the organic phase, and if the pH value is lowered, the reaction of Formula 4 proceeds in reverse, and the metal ions extracted into the organic phase are easily extracted back into the aqueous phase.

[0066] Since the pH value of extraction varies depending on the type of metal ions, in the solvent extraction process using an acidic extractant, the target element and impurity elements are separated by controlling the pH value.

[0067] nR org +M n+ aq →MR norg +nH + aq (Formula 4)

[0068] Here, RH in the formula represents an acidic extractant, M n+ represents n-valent metal ions, org represents organic phase, and aq represents aqueous phase.

[0069] Therefore, in the first solvent extraction step S1, it is more preferred to adjust the pH of the cobalt chloride solution to 1.5 to 3.0. In this pH range, the extraction rates of zinc, manganese and calcium tend to be higher than the extraction rate of cobalt, and these impurity elements can be extracted into the organic phase and separated from cobalt by leaving cobalt in the aqueous phase.

[0070] When the pH value is less than 1.5, the extraction rate of these impurities is low and it is difficult to separate them from cobalt. When the pH value exceeds 3.0, the extraction rate of cobalt also increases, and the separation from impurities decreases. When the pH value is adjusted to 1.5-3.0, there is also a situation where part of the cobalt is extracted, but the organic phase after extraction can also be contacted with a hydrochloric acid solution with a pH value lower than that during extraction to reversely extract the cobalt and recover it, thereby reducing the loss of cobalt.

[0071] Furthermore, when the organic phase is brought into contact with an acidic solution having a pH value of 1 or less, most of the extracted metal ions can be back-extracted into the aqueous phase, and the organic phase after the back-extraction can be reused.

[0072] (Decoppering process S2)

[0073] based on Figure 2 , the copper removal step S2 is described.

[0074] The copper removal step S2 is performed by adding a sulfidizing agent to the cobalt chloride solution after the first solvent extraction step S1. Furthermore, an oxidizing agent and a neutralizing agent are added to adjust the redox potential of the cobalt chloride solution to -100 to 200 mV (Ag / AgCl electrode standard) and the pH value to 1.3 to 3.0.

[0075] Through this step, a precipitate of copper sulfide is generated and separated from the cobalt chloride solution, thereby obtaining a cobalt chloride solution from which copper has been removed.

[0076] The copper in the cobalt chloride solution is removed from the solution by forming a copper sulfide precipitate according to the following formula 1, formula 2 or formula 3.

[0077] CuCl2+H2S→CuS↓+2HCl (Formula 1)

[0078] CuCl2+Na2S→CuS↓+2NaCl (Formula 2)

[0079] CuCl2+NaHS→CuS↓+NaCl+HCl (Formula 3)

[0080] In the copper removal step S2, if the redox potential of the cobalt chloride solution is adjusted to -100 to 200 mV (Ag / AgCl electrode standard) and the pH value is adjusted to 1.3 to 3.0 in advance, copper can be sufficiently removed in the form of sulfide and coprecipitation of cobalt can be suppressed.

[0081] If the redox potential exceeds 200 mV, the removal of copper in the solution is insufficient, and if the redox potential is less than -100 mV, the amount of coprecipitation of cobalt increases, which is not preferred. In addition, when the pH value is less than 1.3, the removal of copper in the solution is insufficient, and the filterability of the generated sulfide precipitate deteriorates. When the pH value exceeds 3.0, the amount of cobalt coprecipitation increases with the removal of copper, which is not preferred.

[0082] The above-mentioned redox potential can be adjusted by adjusting the amount of the sulfiding agent added. The sulfiding agent is not particularly limited, and hydrogen sulfide gas, sodium sulfide or sodium hydrosulfide crystals or aqueous solutions, etc. can be used.

[0083] In addition, when hydrogen sulfide or sodium hydrosulfide is used as a sulfiding agent, the pH value is adjusted by adjusting the amount of the sulfiding agent added and adding a neutralizing agent. The neutralizing agent is not particularly limited, and alkali salts such as sodium hydroxide, calcium hydroxide, sodium carbonate, and cobalt carbonate can be used. In addition, when the oxidation-reduction potential is lower than the desired value due to the addition of a sulfiding agent, it can be adjusted by adding an oxidizing agent. For example, it can be adjusted by introducing air into the solution and stirring it, or by adding a hydrogen peroxide solution.

[0084] (Second solvent extraction step S3)

[0085] based on Figure 2 , Figure 4 and Figure 5 , the second solvent extraction step S3 is described.

[0086] The second solvent extraction step S3 is a step in which the cobalt chloride solution that has passed the above-mentioned copper removal step S2 is contacted with an organic solvent containing a carboxylic acid-based extractant to extract cobalt into the organic solvent (hereinafter referred to as the cobalt extraction step S31), and then a solvent recovery treatment S32 for separating and recovering the carboxylic acid-based extractant from the cobalt chloride solution after the cobalt is extracted, and a step of reversely extracting cobalt with sulfuric acid (hereinafter referred to as the cobalt reverse extraction step S33) are carried out in parallel to obtain a cobalt sulfate solution.

[0087] As the organic solvent, a solvent obtained by diluting a carboxylic acid-based extractant with a diluent can be used. Examples of the carboxylic acid-based extractant include versatic acid and cyclohexane acid. These are acidic extractants having a COOH group.

[0088] When extracting metal ions, carboxylic acid extractants release protons corresponding to the metal valence into the aqueous phase, and the metal ions are coordinated to the carbonyl oxygen. Most carboxylic acids form dimers and trimers through hydrogen bonds in non-polar solvents. In addition, when extracting metal ions, there are cases where carboxylic acids that have not been acid-dissociated are coordinated to remove the hydration water coordinated to the metal ions. For example, the hexacoordinated divalent metal ion M 2+The reaction of extraction by the carboxylic acid extractant R2H2 of the dimer is shown in Formula 5.

[0089] [M(H2O)6] 2+ aq +3(R2H2) org

[0090] →(MR2·4RH) org +2H + aq +6H2O aq (Formula 5)

[0091] Here, org in the formula represents an organic phase, and aq represents an aqueous phase.

[0092] (Cobalt extraction step S31)

[0093] In the cobalt extraction step S31, an alkali solution is added as a neutralizer to the cobalt chloride solution after copper, zinc, manganese and calcium are removed to adjust the pH value to 5.0 to 7.0. If the pH value is within this range, cobalt can be extracted into the organic phase after contact with an organic solvent containing a carboxylic acid extractant.

[0094] At this time, magnesium is not extracted and remains in the aqueous phase. When the pH value is less than 5, it is difficult to extract cobalt, while when the pH value exceeds 7, the solubility of cobalt decreases and precipitation may occur.

[0095] In addition, as an alkaline solution, specifically, a solution of sodium hydroxide or potassium hydroxide can be used.

[0096] In order to prevent oxidation during extraction, bubbling may be performed using an inert gas such as nitrogen, argon or carbon dioxide.

[0097] (Solvent recovery process S32 and cobalt reverse extraction process S33)

[0098] like Figure 2 As shown, after the cobalt extraction step S31, the solvent recovery process S32 and the cobalt reverse extraction step S33 are carried out in parallel.

[0099] (Solvent recovery process S32)

[0100] In the Figure 4 In the cobalt extraction step S31 shown, the residual liquid after the cobalt is extracted, that is, the cobalt chloride solution (aqueous phase), a part of the carboxylic acid extractant will be dissolved therein. This will cause the loss of the extractant, and when the aqueous phase is subjected to drainage treatment and discharged to the sea, etc., it will also cause an impact on the environment caused by TOC (total organic carbon) of the extractant, so it is not preferred. For this reason, it is advisable to perform a solvent recovery process S32 to separate and recover the carboxylic acid extractant.

[0101] like Figure 5 As shown, the solvent recovery process S32 is a process of contacting the cobalt chloride solution (residue) after cobalt extraction with any one or more of the organic solvent, carboxylic acid extractant, and diluent after reverse extraction, and adding a neutralizer or acid to adjust the pH value to 2.0 or more and 4.0 or less, and separating and recovering the carboxylic acid extractant in the cobalt chloride solution. Figure 4 As shown, the solvent recovery process S32 is performed on the residual liquid in the cobalt extraction process S31 using the organic solvent (extractant) obtained in the cobalt reverse extraction process S33.

[0102] By performing the solvent recovery treatment S32, it is possible to prevent the loss of the organic solvent and to suppress the environmental load caused by the wastewater (the increase in TOC concentration caused by the dissolution of the carboxylic acid-based extractant in the aqueous phase).

[0103] (Cobalt reverse extraction step S33)

[0104] like Figure 4 As shown, in the cobalt reverse extraction step S33, the cobalt extracted into the carboxylic acid extractant obtained in the cobalt extraction step S31 is contacted with a sulfuric acid solution, and the pH value is adjusted to 2.0 to 4.5. Thus, the cobalt can be reversely extracted into the sulfuric acid solution. In this way, a high-purity cobalt sulfate solution can be obtained.

[0105] Even if the pH value is less than 2, reverse extraction can be performed, but even if the pH value is reduced too much, the recovery amount will not change much, and the obtained effect is small. On the other hand, since the reverse extraction amount of trace impurities extracted at a pH value lower than cobalt increases, it is not preferred. Furthermore, there are also issues such as consuming reagent costs, so the pH value is preferably above 2.0. On the other hand, when the pH value exceeds 4.5, the cobalt reverse extraction rate decreases, and the recovery amount of cobalt decreases, so it is not preferred.

[0106] Furthermore, since the extracted organic phase is mixed with a fine aqueous phase even after phase separation, a washing step for removing the aqueous phase may be added before reverse extraction. The aqueous phase in the washing step may be, for example, a cobalt sulfate solution. In addition, the organic solvent after reverse extraction obtained in the cobalt reverse extraction step S33 may be reused as the organic solvent used in the solvent recovery process S32.

[0107] By the above method, a high-purity cobalt sulfate solution with less impurities can be produced.

[0108] (Crystallization Step S4)

[0109] based on Figure 1 The crystallization step S4 will be described.

[0110] In the crystallization step S4, crystals of cobalt sulfate are precipitated from the cobalt sulfate solution obtained in the second solvent extraction step S3. The crystallization method is not particularly limited, and a common crystallization method can be used.

[0111] For example, a method of obtaining a crystal by placing a cobalt sulfate solution in a crystallization tank and performing crystallization in the crystallization tank can be cited. The crystallization tank is a method of precipitating crystals by evaporating the water in the cobalt sulfate solution under a specific pressure, and for example, a rotary evaporator or a twin-screw type crystallization tank can be used. The internal pressure is reduced by a vacuum pump or the like, and the flask is rotated in the rotary evaporator while crystallization is performed, and a twin-screw propeller is used to stir while crystallization is performed. Furthermore, in the crystallization tank, a slurry in which cobalt sulfate crystals are mixed in the cobalt sulfate solution is made.

[0112] The slurry discharged from the crystallization tank is separated into cobalt sulfate crystals and mother liquor by a filter or a centrifugal separator, etc. Then, the cobalt sulfate crystals are dried in a dryer to remove moisture.

[0113] By using the above method, cobalt sulfate crystals can be produced from a cobalt sulfate solution. Of course, since the cobalt sulfate solution has fewer impurities and higher purity, the obtained cobalt sulfate crystals also become high-purity crystals with fewer impurities.

[0114] [Example]

[0115] Hereinafter, examples of the present invention will be shown and described in more detail, but the present invention is not limited to the following examples at all.

[0116] (Example 1)

[0117] (First solvent extraction step S1)

[0118] Prepare an organic phase diluted with a diluent (trade name: Techlean N20, manufactured by JX Nippon Mining and Energy Co., Ltd.) in such a manner that the concentration of an alkylphosphoric acid-based extractant (trade name: D2EHPA, manufactured by Daihachi Chemical Industry Co., Ltd.) becomes 40% by volume. 0.9L of an aqueous phase consisting of a "cobalt chloride solution consisting of the composition shown in the original solution A in Table 1" is mixed with 1.8L of an organic phase, and a sodium hydroxide solution is added to adjust the pH value to 1.7 to extract impurities. Repeat the same extraction operation with 0.9L of the extracted aqueous phase and 1.8L of a new organic phase, and perform a total of 3 extraction operations. As a result, a cobalt chloride solution with the composition shown in B after the 1SX in Table 1 is obtained. The concentrations of zinc, manganese and calcium are all below 0.001g / L, and these impurities are successfully separated and removed.

[0119] (Decoppering process S2)

[0120] After adjusting the pH value of the cobalt chloride solution 0.9 L obtained in the first solvent extraction step S1 to 2.5 by adding a sodium hydroxide solution, a sodium hydrogen sulfide solution was added as a sulfiding agent, and the oxidation-reduction potential was adjusted to -50 mV (Ag / AgCl electrode standard) to generate a precipitate of copper sulfide. The precipitate was separated and removed by a filter to obtain a filtrate having a composition shown in Table 1 after sulfidation C. The copper concentration was less than 0.001 g / L, and copper was successfully separated and removed.

[0121] (Second solvent extraction step S3)

[0122] An organic phase was prepared by diluting a carboxylic acid extractant (trade name: Versatic Acid 10, manufactured by Oxalis Chemicals Ltd.) with a diluent (Techlean N20) to a concentration of 30% by volume. 0.44 L of an aqueous phase consisting of the cobalt chloride solution obtained in the copper removal step S2 was mixed with 1 L of the organic phase, and a sodium hydroxide solution was added to adjust the pH to 6.5, thereby extracting cobalt into the organic phase.

[0123] 0.6 L of the extracted organic phase was mixed with 0.6 L of a cobalt chloride solution having a cobalt concentration of 10 g / L, and the aqueous phase mixed in the extracted organic phase was washed. Next, the organic phase was mixed with 0.09 L of pure water, sulfuric acid was added, the pH value was adjusted to 4, and cobalt was reversely extracted. As a result, a cobalt sulfate solution of the composition shown in the second SX after D of Table 1 was obtained. The magnesium concentration was less than 0.001 g / L, and magnesium was successfully separated and removed.

[0124] Through the above method, a high-purity cobalt sulfate solution is obtained.

[0125] [Table 1]

[0126] element Co Cu Zn Mn Ca Mg Stock Solution A 85 0.01 0.15 0.098 3.9 0.042 1stSX Post B 64 0.002 <0.001 <0.001 0.001 0.028 After vulcanization C 57 <0.001 <0.001 <0.001 0.001 0.026 2ndSX Rear D 111 <0.001 <0.001 <0.001 <0.001 <0.001

[0127] (Unit: g / L)

[0128] (Crystallization Step S4)

[0129] The cobalt sulfate solution was placed in a rotary evaporator, the inside was depressurized with a vacuum pump, and the temperature was maintained at 40°C. The flask was rotated while the water was evaporated, thereby precipitating cobalt sulfate crystals. After solid-liquid separation, the obtained cobalt sulfate crystals were dried with a dryer. As a result, high-purity cobalt sulfate crystals were obtained as shown in Table 2.

[0130] [Table 2]

[0131] element Co Cu Zn Mn Ca Mg concentration 22 <1 <1 <5 <10 <1

[0132] (Unit: Cobalt is %, other elements are ppm)

[0133] (Example 2)

[0134] In the copper removal step S2, the redox potential was adjusted to 150 mV (Ag / AgCl electrode reference), and in the second solvent extraction step S3, 0.44 L of the aqueous phase obtained by diluting the cobalt chloride solution obtained in the copper removal step S2 by 2 times with pure water was mixed with the organic phase, 0.6 L of the extracted organic phase was mixed with 0.6 L of the cobalt chloride solution with a cobalt concentration of 10 g / L, the aqueous phase mixed in the extracted organic phase was washed, and the organic phase was mixed with 0.08 L of pure water, sulfuric acid was added to adjust the pH to 4, and cobalt was reversely extracted. Except for this, a cobalt sulfate solution was obtained in the same manner as in Example 1.

[0135] The composition at this time is shown in Table 3. As shown in 2SX after D in Table 3, a high-purity cobalt sulfate solution was successfully obtained.

[0136] [Table 3]

[0137] element Co Cu Zn Mn Ca Mg Stock Solution A 85 0.01 0.15 0.098 3.9 0.042 1stSX Post B 64 0.002 <0.001 <0.001 0.001 0.028 After vulcanization C 58 <0.001 <0.001 <0.001 0.001 0.027 2ndSX Rear D 92 <0.001 <0.001 <0.001 <0.001 <0.001

[0138] (Unit: g / L)

[0139] Next, crystallization was carried out in the same manner as in Example 1, and as a result, high-purity cobalt sulfate crystals as shown in Table 4 were obtained.

[0140] [Table 4]

[0141] element Co Cu Zn Mn Ca Mg concentration 22 <1 <1 <5 <10 <1

[0142] (Unit: Cobalt is %, other elements are ppm)

[0143] (Example 3)

[0144] A cobalt sulfate solution was obtained in the same manner as in Example 1 except that the solvent recovery process S32 was performed. In the solvent recovery process S32, sulfuric acid was added to the cobalt chloride solution having a pH value of 6.5 after cobalt was extracted in the cobalt extraction step S31 to adjust the pH value to 2 to 4, and the carboxylic acid extractant was separated and recovered.

[0145] Then, the TOC concentration in the cobalt chloride solution was measured using a known method. As shown in Table 5, by reducing the pH to 4 or less, the TOC contained in the solution of 260 mg / l was reduced to about 100 mg / l, that is, the carboxylic acid-based extractant was successfully separated from the cobalt chloride solution. As a result, the loss of the extractant was successfully suppressed, and the environmental load when the cobalt chloride solution after extraction was treated as wastewater and discharged to the sea, etc. was successfully reduced.

[0146] [Table 5]

[0147] Cobalt chloride solution Before pH adjustment [pH 6.5] pH = 4 pH = 3 pH = 2 TOC[mg / l] 260 106 98 98

[0148] According to the results of Examples 1, 2 and 3 above, it can be seen that, according to the present invention, high-purity cobalt sulfate with impurities sufficiently removed can be obtained. In addition, it can be seen that, if the solvent recovery process S32 is performed, the loss of the extractant can be suppressed, or the environmental load when the cobalt chloride solution after extraction is treated for drainage and discharged to the sea or the like can be reduced.

[0149] Industrial Applicability

[0150] The high-purity cobalt sulfate crystals obtained by the present invention can be used for various purposes besides being a raw material for lithium-ion secondary batteries.

[0151] Description of Reference Numerals

[0152] S1: First solvent extraction step.

[0153] S2: copper removal process.

[0154] S3: Second solvent extraction step.

[0155] S4: Crystallization step.

[0156] S31: Cobalt extraction process.

[0157] S32: Solvent recovery process.

[0158] S33: Cobalt reverse extraction process.

Claims

1. A method for producing cobalt sulfate, in, The method for producing cobalt sulfate sequentially implements the following steps: A first solvent extraction step, in which a cobalt chloride solution containing one or more impurities of copper, zinc, manganese, calcium and magnesium is contacted with an organic solvent containing an alkylphosphoric acid-based extractant, the pH value of the cobalt chloride solution is adjusted to 1.5 to 3.0, and zinc, manganese and calcium as impurities are extracted into the organic solvent to be separated and removed; a copper removal step, in which a sulfiding agent is added to the cobalt chloride solution that has undergone the first solvent extraction step, an oxidant and a neutralizing agent are added to the cobalt chloride solution to which the sulfiding agent is added, the oxidation-reduction potential is adjusted to -100 to 200 mV based on the Ag / AgCl electrode, and the pH value is adjusted to 1.3 to 3.0, a precipitate of copper sulfide is generated, and the precipitate is separated and removed; and A second solvent extraction step is performed, in which the cobalt chloride solution that has undergone the copper removal step is contacted with an organic solvent containing neodecanoic acid, an alkali solution is added, the pH value is adjusted to 5.0 to 7.0, and cobalt is extracted into the organic solvent. Then, a sulfuric acid solution is contacted with the organic solvent, the pH value is adjusted to 2.0 to 4.5, and cobalt is reversely extracted into the sulfuric acid solution to obtain a cobalt sulfate solution.

2. The method for producing cobalt sulfate according to claim 1, in, The alkylphosphoric acid-based extractant used in the first solvent extraction step is bis(2-ethylhexyl) hydrogen phosphate.

3. The method for producing cobalt sulfate according to claim 1, in, The cobalt sulfate solution obtained through the second solvent extraction step is subjected to a crystallization step to obtain cobalt sulfate crystals.

4. The method for producing cobalt sulfate according to claim 1 or 2, in, The second solvent extraction step includes a solvent recovery process, which is a process in which the cobalt chloride solution after cobalt is extracted is contacted with an organic solvent after back-extraction of cobalt into a sulfuric acid solution, the pH value is adjusted to 2.0 or more and 4.0 or less, and neodecanoic acid in the cobalt chloride solution is separated.