A magnetic catalytic adsorbent for flue gas demercuration and denitrification, and its preparation method and application
By using magnetic catalytic adsorbents in the flue gas of coal-fired power plants, combined with EVS-10 molecular sieve and manganese oxide, the problem of synergistic removal of Hg0 and NOx is solved, achieving efficient removal and recycling, and reducing costs and pollution.
Patent Information
- Application Number
- CN202111273176.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Existing technology is difficult to effectively remove Hg0 and nitrogen oxides from the flue gas of coal-fired power plants, and the catalyst recycling efficiency is low, resulting in pollutant emissions and secondary pollution problems.
Using magnetic catalytic adsorbent, including EVS-10 molecular sieve as a carrier, loading nano-Fe3O4 particles and silicon oxide layer, combined with manganese oxide active components, the catalytic performance is improved through oxidation reaction, and the coordinated removal of Hg0 and NOx is achieved.
Efficient removal of Hg0 and NOx is achieved, with mercury removal efficiency reaching over 91% and denitration efficiency reaching over 83%. The catalyst is easy to recycle, reducing fly ash secondary pollution and usage costs.
Smart Images

Figure BDA0003329329340000131 
Figure BDA0003329329340000132 
Figure BDA0003329329340000141
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of environmental protection and air pollution control, and in particular to a magnetic catalytic adsorbent for flue gas demercurization and denitrification, and a preparation method and application thereof. Background Art
[0002] Mercury is a toxic heavy metal that poses a serious threat to human health and the ecological environment. Coal-fired power plants are considered the world's largest source of anthropogenic mercury emissions. Therefore, it is imperative to research technologies for efficiently removing mercury from coal-fired power plant flue gases. Coal-fired power plants are considered one of the most important sources of anthropogenic mercury emissions. Mercury in flue gas is mainly present in the form of Hg 2+ 、Hg p and Hg 0 There are three forms, Hg 2+ It is soluble in water and can therefore be removed efficiently by the wet desulfurization device of the pollutant control equipment; Hg in the flue gas p Since it combines with fly ash, it can be removed by particulate matter control equipment such as bag filters or electrostatic precipitators; however, Hg 0 It is insoluble in water and volatile, and is quite stable at low temperatures. It is difficult to be removed by the existing pollutant control equipment in power plants and is directly discharged into the atmosphere. Therefore, the key to removing mercury from flue gas of coal-fired power plants is to control Hg 0 emissions.
[0003] At present, the two main research directions of mercury removal are adsorbent demercuration and catalytic oxidation demercuration: Adsorbent demercuration is to remove Hg 0 Through physical or chemical adsorption to the adsorbent surface, and then removed by the particulate matter control equipment; catalytic oxidation demercuration is to remove Hg 0 Efficient oxidation to Hg 2+ , and is subsequently removed by the wet desulfurization unit. EVS-10 is a molecular sieve in which vanadium completely replaces the titanium in the titanium silicate molecular sieve ETS-10. It is primarily composed of vanadium oxide octahedra and silicon oxide tetrahedra, linked by common corner oxygen atoms to form a three-dimensional network structure. This molecular sieve exhibits a certain catalytic capacity, similar to industrial vanadium-supported catalysts, and can catalyze the oxidation of elemental mercury. However, this material's catalytic efficiency for mercury oxidation is only approximately 48%, which is relatively low.
[0004] In addition to elemental mercury, nitrogen oxides are also a common air pollutant produced by coal combustion, which can cause acid rain and greenhouse effect. x) accounts for over 95% of NO in coal-fired flue gas, so the key to removing nitrogen oxides is removing NO. Currently, the most effective and widely used technology for removing NO from coal-fired flue gas is NH3 selective catalytic reduction (SCR). The SCR catalysts currently under study are primarily prepared by loading metal oxides such as V2O5, CuO, Cr2O3, CeO2, Fe2O3, MnOx, and Co2O3 onto carriers such as Al2O3, SiO2, TiO2, ZrO2, carbon materials, and molecular sieves. Considering that the EVS-10 molecular sieve has a certain ability to remove mercury, but its catalytic denitrification performance is poor (only 14% removal efficiency), it cannot achieve the goal of simultaneous mercury and nitrogen removal.
[0005] In addition, catalyst recycling is also a problem. How to effectively recycle catalysts and avoid secondary pollution of fly ash has also attracted widespread attention. Summary of the Invention
[0006] The purpose of the present disclosure is to provide a magnetic catalytic adsorbent for flue gas demercurization and denitrification, and its preparation method and application. The magnetic catalytic adsorbent can achieve the synergistic removal of mercury and nitrogen oxides and is easy to recycle.
[0007] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides a magnetic catalytic adsorbent for flue gas demercurization and denitrification, wherein the magnetic catalytic adsorbent includes a carrier, magnetic particles and an active component; the magnetic particles include nano-Fe3O4 particles and a silicon oxide layer coated on the surface of the nano-Fe3O4 particles, and the active component is loaded on the carrier; the carrier includes EVS-10 molecular sieve, and the active component includes manganese oxide.
[0008] Optionally, based on the total weight of the catalytic adsorbent, the mass fraction of the magnetic particles is 5-50 weight %, the mass fraction of the carrier is 35-94 weight %, and the mass fraction of the active component is 1-15 weight %.
[0009] The second aspect of the present disclosure provides a method for preparing the magnetic catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps:
[0010] (1) mixing a magnetic EVS-10 molecular sieve, a manganese source, and water to obtain a raw material mixture;
[0011] (2) adding an alkaline solution and an oxidant to the raw material mixture to contact and perform an oxidation reaction;
[0012] The magnetic EVS-10 molecular sieve comprises the EVS-10 molecular sieve and the magnetic particles.
[0013] Optionally, the method further comprises preparing the magnetic EVS-10 molecular sieve by the following steps:
[0014] a. mixing Fe3O4 particles, a silicate solution, and water, and then adding an acid to adjust the pH, preferably to 9.3 to 9.7, to obtain a first mixture;
[0015] b. heating and cooling the first mixture, and then performing a first separation to obtain a first solid product having magnetic properties;
[0016] c. Dispersing the EVS-10 molecular sieve and the first solid product in a solvent, performing a second separation to remove the solvent; and performing a calcination treatment to obtain the magnetic EVS-10 molecular sieve.
[0017] Optionally, in step a, the weight ratio of the Fe3O4 particles, silicate and water is (0.4-1):1:(26-60);
[0018] The silicate is preferably sodium silicate; further preferably, the concentration of the silicate solution is 0.5 to 3 mol / L;
[0019] The acid is preferably hydrochloric acid or sulfuric acid; more preferably, the concentration of the acid is 0.1 to 1 mol / L;
[0020] Optionally, the acid is added to adjust the pH to 9.3-9.7;
[0021] Optionally, step a comprises: dispersing the suspension of the Fe3O4 particles and deionized water under ultrasonic treatment and / or mechanical stirring conditions, and then adding the silicate solution.
[0022] Optionally, step b includes:
[0023] The first mixture is kept at 30-45°C for 2-4 hours; then heated to 85-95°C, kept for 1-2 hours; then cooled to 20-40°C;
[0024] Optionally, the first separation is performed using a magnetic separation device.
[0025] Optionally, in step c, the solvent is selected from one or more of toluene, acetone and ethyl acetate, preferably toluene;
[0026] Optionally, step c further comprises: adding the carrier molecular sieve to the solvent and ultrasonically mixing, then adding the first solid product and continuing ultrasonically mixing; then standing the obtained suspension to separate layers, removing the upper layer of solvent, and then removing the residual solvent under vacuum;
[0027] In step c, the conditions for the calcination treatment include: a calcination temperature of 250 to 350° C. and a calcination time of 1 to 2 hours.
[0028] Optionally, in step (1), the weight ratio of the magnetic EVS-10 molecular sieve, the manganese source and water is (0.015-0.1): (0.2-0.3): 1;
[0029] The manganese source is a water-soluble manganese salt, preferably one or more selected from manganese acetate, manganese chloride and manganese nitrate.
[0030] Optionally, the raw material mixture in step (1) further comprises a dispersing aid; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, preferably polymethacrylic acid;
[0031] Preferably, the weight ratio of the dispersing aid to the manganese source is (0.7-3): (2-6);
[0032] Optionally, step (1) further comprises: mixing the manganese source, water and the optional dispersing aid, performing ultrasonic treatment and adding the magnetic EVS-10 molecular sieve to obtain the raw material mixture.
[0033] Optionally, in step (2), the alkaline solution is a sodium hydroxide solution; preferably, the volume ratio of the sodium hydroxide solution to the water in step (1) is 0.3 to 0.7:1;
[0034] The oxidant is hydrogen peroxide, and more preferably, the concentration of the hydrogen peroxide is 25 to 35% by weight.
[0035] Optionally, in step (2), the conditions of the oxidation reaction include: a reaction temperature of 40 to 80° C., and a reaction time of 0.5 to 2 h;
[0036] Optionally, step (2) further comprises: filtering, washing, drying, and then screening the oxidation reaction product; wherein the drying temperature of the oxidation reaction product is 70 to 110°C.
[0037] The third aspect of the present disclosure provides an application of the magnetic catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0038] Through the above technical solution, the present disclosure provides a magnetic catalytic adsorbent for flue gas demercurization and denitrification, the catalytic adsorbent includes magnetic particles with magnetism, which are easy to recycle, avoid secondary pollution of fly ash, and have low use costs; the catalytic adsorbent uses EVS-10 molecular sieve as a carrier to load highly dispersed manganese oxide active components, and has good demercurization and denitrification performance; and the EVS-10 molecular sieve framework contains vanadium atoms, which can also act as active components, further improving the catalytic oxidation performance of the adsorbent. The magnetic catalytic adsorbent provided by the present disclosure has good process adaptability and compatibility, is suitable for use in series with dust removal and desulfurization equipment, and is particularly suitable for upgrading and renovating old enterprises with desulfurization and dust removal equipment for demercurization, reducing equipment installation and use costs, and has industrial application prospects.
[0039] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0040] The following describes the specific embodiments of the present disclosure in detail. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure and are not intended to limit the present disclosure.
[0041] In a first aspect, the present disclosure provides a magnetic catalytic adsorbent for demercuration and denitrification of flue gas, the magnetic catalytic adsorbent comprising a carrier, magnetic particles, and an active component; the magnetic particles comprising nano-Fe3O4 particles and a silicon oxide layer coated on the surface of the nano-Fe3O4 particles, the active component being loaded on the carrier; the carrier comprising EVS-10 molecular sieve, and the active component comprising manganese oxide.
[0042] The present disclosure provides a catalytic adsorbent, including magnetic particles with magnetism, which are easy to recycle and reuse, avoid secondary pollution of fly ash, and have low use costs. The catalytic adsorbent uses EVS-10 molecular sieve as a carrier to load a highly dispersed manganese oxide active component, which has good demercuration and denitrification performance. In addition, the EVS-10 molecular sieve framework contains vanadium atoms, which can also act as active components, further improving the catalytic oxidation performance of the adsorbent. The magnetic catalytic adsorbent provided by the present disclosure has good process adaptability and compatibility, is suitable for use in series with dust removal and desulfurization equipment, and is particularly suitable for upgrading and renovating old enterprises with desulfurization and dust removal equipment for demercuration, reducing equipment installation and use costs, and has prospects for industrial application.
[0043] The present invention uses nano-Fe3O4 particles coated with a silicon oxide layer as magnetic particles and EVS-10 molecular sieve to form a catalytic adsorbent. The silicon oxide layer can not only protect the nano-Fe3O4 particles from maintaining their magnetism under complex conditions such as high temperature and acidity, but also play a role in connecting the molecular sieve. In this catalytic adsorbent, EVS-10 molecular sieve is used as a carrier. The molecular sieve skeleton contains vanadium atoms and is loaded with the active component manganese oxide. The vanadium atoms and manganese oxide enable the catalytic adsorbent to catalyze the oxidation of Hg 0 , can also catalytically reduce NOx, achieving Hg 0 The synergistic and efficient removal of NOx can achieve a mercury removal efficiency of over 91% and a denitrification efficiency of over 83%.
[0044] In one embodiment, based on the total weight of the catalytic adsorbent, the mass fraction of the magnetic particles is 5 to 50% by weight, the mass fraction of the carrier is 35 to 94% by weight, and the mass fraction of the active component is 1 to 15%. When the contents of the components in the catalytic adsorbent provided by the present disclosure are within the ranges of this embodiment, the resulting catalytic adsorbent can achieve good synergistic removal of elemental mercury and nitrogen oxides, while also achieving high catalytic adsorbent recovery efficiency.
[0045] The magnetic particles disclosed herein are specifically nano-Fe₃O₄ particles coated with a SiO₂ layer. Specifically, the magnetic particles have a particle size of 50 to 200 nm. The SiO₂ layer content can vary widely, such that the final mass fraction of the magnetic particles in the catalytic adsorbent is 5 to 50% by weight.
[0046] The carrier is an EVS-10 molecular sieve; in one embodiment, based on the molar amount of elements, the molar ratio of Si:Na:K:V in the EVS-10 molecular sieve is 3.92:1.39:0.48:1.
[0047] The second aspect of the present disclosure provides a method for preparing the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps:
[0048] (1) mixing a magnetic EVS-10 molecular sieve, a manganese source, and water to obtain a raw material mixture;
[0049] (2) adding an alkaline solution and an oxidant to the raw material mixture to contact and perform an oxidation reaction;
[0050] The magnetic EVS-10 molecular sieve comprises the EVS-10 molecular sieve and the magnetic particles.
[0051] During experiments, the inventors discovered a method for loading manganese oxide that differs from the traditional impregnation and calcination process. First, a manganese source and magnetic EVS-10 molecular sieve are dispersed in water. The raw material mixture is then oxidized to the manganese source under alkaline conditions and in the presence of an oxidant (such as hydrogen peroxide). This oxidizes the manganese source onto the surface of the EVS-10 molecular sieve to form a highly dispersed manganese oxide active component. In actual preparation, manganese oxide may also be present on the magnetic particles, resulting in a magnetic catalytic adsorbent with synergistic mercury and nitrogen removal properties.
[0052] The EVS-10 molecular sieve used in the present disclosure can be prepared according to existing methods, for example, it can be prepared by the method disclosed in the document ZijianZhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8.
[0053] In a specific embodiment, the EVS-10 molecular sieve used in the present disclosure can be prepared by a hydrothermal method, specifically comprising: dissolving sodium silicate in deionized water; then adding NaOH, KCl, NaF and NaCl to the solution to obtain solution A. VOSO4 is then dissolved in deionized water to obtain solution B. Solution A and solution B are mixed and stirred, and aged at room temperature. The aged mixture is transferred to an autoclave for further aging. The synthesized product is washed with deionized water and dried to obtain the EVS-10 molecular sieve. During the preparation process, the amount of each reactant and the reaction conditions can be adjusted according to actual needs.
[0054] In one embodiment, the method further comprises preparing the magnetic EVS-10 molecular sieve by the following steps:
[0055] a. mixing Fe3O4 particles, a silicate solution, and water, and then adding an acid to adjust the pH, preferably to 9.3 to 9.7, to obtain a first mixture;
[0056] b. heating and cooling the first mixture, and then performing a first separation to obtain a first solid product having magnetic properties;
[0057] c. Dispersing the EVS-10 molecular sieve and the first solid product in a solvent, performing a second separation to remove the solvent; and performing a calcination treatment to obtain the magnetic EVS-10 molecular sieve.
[0058] The present invention first coats the Fe3O4 nanoparticles with a SiO2 thin layer through the above steps a and b. The SiO2 thin layer can not only protect the Fe3O4 nanoparticles to maintain their magnetism under complex conditions such as high temperature and acidity, but also play a connecting role. In step c, the high-temperature calcination process firmly bonds with the EVS-10 molecular sieve to obtain the magnetic EVS-10 molecular sieve.
[0059] Furthermore, the present invention first synthesizes the magnetic EVS-10 molecular sieve through the above steps a to c and then loads the manganese oxide active component, which can ensure that the loading of manganese oxide is not affected, and further ensure that the final catalytic adsorbent has good magnetic properties and high mercury removal and denitrification performance.
[0060] In one embodiment, in step a, the weight ratio of the Fe3O4 particles, silicate and water is (0.4-1):1:(26-60); the silicate includes sodium silicate; further preferably, the concentration of the silicate solution is 0.5-3 mol / L;
[0061] The acid is preferably hydrochloric acid or sulfuric acid; more preferably, the concentration of the acid is 0.1 to 1 mol / L;
[0062] Optionally, the acid is added to adjust the pH to 9.3-9.7;
[0063] Optionally, step a comprises: subjecting the suspension of the Fe3O4 particles and deionized water to ultrasonic treatment and / or mechanical stirring treatment simultaneously, and then adding the silicate solution.
[0064] In one embodiment, step b comprises: keeping the first mixture at 30-45°C for 2-4 hours; then heating it to 85-95°C and keeping it for 1-2 hours; then cooling it to 20-40°C;
[0065] Optionally, the first separation includes separation using a magnetic separation device.
[0066] In one embodiment, in step c, the solvent is selected from one or more of toluene, acetone, and ethyl acetate, preferably toluene. The present disclosure uses an organic solvent such as toluene rather than an aqueous solution to disperse the EVS-10 molecular sieve and the Fe3O4 nanoparticles coated with a thin SiO2 layer, thereby preventing the SiO2 layer from dissolving and migrating to the molecular sieve surface, thereby clogging the molecular sieve pores.
[0067] In an optional embodiment, step c further comprises: adding the carrier molecular sieve to the solvent and ultrasonically mixing, then adding the first solid product and continuing ultrasonically mixing; then standing the obtained suspension to separate layers, removing the upper layer solvent, and then removing the residual solvent under vacuum.
[0068] In one embodiment, in step c, the calcination conditions include: a calcination temperature of 250 to 350° C. and a calcination time of 1 to 2 hours.
[0069] In one embodiment, in step (1), the weight ratio of the magnetic EVS-10 molecular sieve, the manganese source and water is (0.015-0.1): (0.2-0.3): 1; the manganese source is a water-soluble manganese salt, preferably one or more of manganese acetate, manganese chloride and manganese nitrate.
[0070] In a preferred embodiment, the raw material mixture in step (1) further comprises a dispersing aid; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, preferably polymethacrylic acid.
[0071] The present invention simultaneously introduces a manganese source and a dispersing aid during the preparation of a catalytic adsorbent. The Mn ions form a complex (chelate) with the dispersing aid, so that even when an alkaline solution (such as sodium hydroxide) is subsequently added to carry out an oxidation reaction under alkaline conditions, precipitation will not occur. The uniformly dispersed Mn ion complex obtained can be stably present in the system, further avoiding agglomeration. After the addition of an oxidant (such as hydrogen peroxide), the manganese ions in the system are oxidized on the surface of the magnetic EVS-10 molecular sieve to form highly dispersed manganese oxide active components, and the dispersion of the manganese oxide active components on the molecular sieve is improved.
[0072] In one embodiment, step (1) further comprises: mixing the manganese source, water and the optional dispersing aid, performing ultrasonic treatment and adding the magnetic EVS-10 molecular sieve to obtain the raw material mixture.
[0073] In one embodiment, the alkaline solution in step (2) is a sodium hydroxide solution; the concentration of the alkaline solution is 25 to 35 mol / L; preferably, the volume ratio of the aqueous solution of sodium hydroxide to the water in step (1) is 0.3 to 0.7:1;
[0074] The oxidant is hydrogen peroxide, and more preferably the concentration of the hydrogen peroxide is 25-35%.
[0075] In one embodiment, in step (2), the conditions of the oxidation reaction include: a reaction temperature of 40 to 80° C., and a reaction time of 0.5 to 2 h;
[0076] Optionally, step (2) further comprises: washing, drying, and then screening the oxidation reaction product; wherein the oxidation reaction product is dried at a temperature of 70 to 110° C. Specifically, a 100-mesh sieve can be used for screening, and the particles under the sieve are used as the catalytic adsorbent.
[0077] The third aspect of the present disclosure provides an application of the catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0078] The present invention is further described below with reference to specific embodiments. However, the scope of protection claimed by the present invention is not limited to the scope described in the embodiments.
[0079] The chemicals used in each example can be obtained through public commercial channels.
[0080] The EVS-10 molecular sieve used in the following examples and comparative examples was prepared according to the method disclosed in the literature Zijian Zhou, Tiantian Cao, et al. “Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas”. Journal of Hazardous Materials, 375 (2019) 1-8.
[0081] In the following examples, 30 wt % hydrogen peroxide means that the mass fraction of H2O2 in the aqueous solution is 30%.
[0082] The “ultrasonic treatment” described in this disclosure refers to the use of a conventional ultrasonic instrument to perform ultrasonic treatment to make the material mixing or dispersion more uniform.
[0083] Example 1
[0084] (1) A suspension of 2 g of Fe3O4 particles and 120 mL of deionized water was simultaneously ultrasonically treated and mechanically stirred at 40°C. 2.23 g of sodium silicate pentahydrate was dissolved in water to prepare 10 mL of a 1 mol / L sodium silicate solution, which was added to the suspension. 0.3 mol / L sulfuric acid was then added dropwise to control the pH of the solution to 9.5 ± 0.2. The solution was heated to 95°C for 3 hours and then heated to 1 hour. The solution was then cooled to room temperature. The SiO2-coated Fe3O4 particles were separated by a magnet, washed twice with deionized water, and dried in a vacuum drying oven.
[0085] (2) 8 g of EVS-10 molecular sieve was mixed with toluene by ultrasonic treatment, and 2 g of Fe3O4 particles coated with SiO2 were added. The ultrasonic treatment was continued. After the suspension was separated, the upper toluene liquid was poured out and the remaining toluene was removed under vacuum. The lower solid was placed in a tube furnace and calcined at 300 ° C for 1 hour under a nitrogen atmosphere. After cooling to room temperature, it was sieved with a 100 mesh screen and the particles under the sieve were taken to obtain magnetic EVS-10 molecular sieve;
[0086] (3) 2.8 g of Mn(CH3COO)2·4H2O and 6.0 g of PMAA were dissolved in 40 mL of deionized water, and 9.0 g of magnetic EVS-10 molecular sieves were added while ultrasonicating for 15 min.
[0087] (4) Slowly add 25 mL of 2 mol / L sodium hydroxide solution, ultrasonically treat for 15 minutes, then add 5 mL of 30 wt% hydrogen peroxide, react at 60°C for 1 hour, filter out the solid sample, repeatedly rinse with ethanol and deionized water to rinse off the residual substances on the surface of the product obtained after the reaction, then dry the sample at 80°C, and finally sieve the dried sample with a 100-mesh sieve, take the sieve particles, and obtain the final magnetic catalytic adsorbent, which is recorded as C-1.
[0088] Comparative Example 1
[0089] A catalytic adsorbent was prepared using steps similar to those in Example 1, except that the EVS-10 molecular sieve was replaced with a commercially available ETS-10 molecular sieve. The remaining preparation steps were the same as in Example 1 to obtain a catalytic adsorbent designated D-1.
[0090] Comparative Example 2
[0091] (1) A suspension of 2 g of Fe3O4 particles and 120 mL of deionized water was mechanically stirred at 40°C, 2.23 g of sodium silicate pentahydrate was dissolved in water to prepare 10 mL of a 1 mol / L sodium silicate solution, which was added to the suspension, and 0.3 mol / L of sulfuric acid was added dropwise to control the pH of the solution to 9.5±0.2. The solution was kept warm for 3 hours and then raised to 95°C, kept warm for 1 hour, and then cooled to room temperature. The Fe3O4 particles coated with SiO2 were separated by a magnet, washed twice with deionized water, and dried in a vacuum drying oven; (2) 8 g of EVS-10 molecular sieve was mixed with toluene by ultrasonic treatment, 2 g of Fe3O4 particles coated with SiO2 were added, and ultrasonic treatment was continued. After the suspension was separated, the upper toluene liquid was poured out, and the remaining toluene was removed under vacuum. The lower layer solid was placed in a tubular furnace and calcined at 300°C for 1 hour under a nitrogen atmosphere. After cooling to room temperature, it was sieved with a 100-mesh sieve. The particles under the sieve were taken to obtain a magnetic EVS-10 molecular sieve, which was recorded as D-2.
[0092] Example 2
[0093] (1) A suspension of 1 g of Fe3O4 particles and 60 mL of deionized water was simultaneously ultrasonically treated and mechanically stirred at 40°C. 2.23 g of sodium silicate pentahydrate was dissolved in water to prepare 20 mL of a 0.5 mol / L sodium silicate solution, which was added to the suspension. 0.2 mol / L hydrochloric acid was then added dropwise to control the pH of the solution to 9.5 ± 0.2. The temperature was kept at 95°C for 3 hours, and the temperature was continued to be kept at 95°C for 1 hour. The solution was then cooled to room temperature. The Fe3O4 particles coated with SiO2 were separated by a magnet, washed twice with deionized water, and dried in a vacuum drying oven.
[0094] (2) 9 g of EVS-10 molecular sieve was ultrasonically mixed with toluene, and 1 g of Fe3O4 particles coated with SiO2 was added. The ultrasonic treatment was continued. After the suspension was separated, the upper toluene liquid was poured out and the remaining toluene was removed under vacuum. The lower solid was placed in a tube furnace and calcined at 300°C for 1 hour under a nitrogen atmosphere. The solid was sieved to less than 100 mesh to obtain a magnetic EVS-10 molecular sieve.
[0095] (3) 0.72 g of MnCl2 and 2.0 g of PMAA were dissolved in 40 mL of deionized water, and 9.5 g of magnetic EVS-10 molecular sieves were added while ultrasonicating for 15 min;
[0096] (4) Slowly add 12 mL of 2 mol / L sodium hydroxide solution, ultrasonically treat for 15 minutes, then add 3 mL of 30 wt% hydrogen peroxide, react at 60°C for 1 hour, filter out the solid sample, and repeatedly rinse with ethanol and deionized water to rinse away the residual substances on the surface of the product obtained after the reaction; then dry the sample at 80°C, and finally sieve the dried sample to below 100 mesh to obtain the final magnetic catalytic adsorbent, which is recorded as C-2.
[0097] Example 3
[0098] A preparation method similar to that of Example 1 was adopted, except that no PMMA dispersing aid was added in step (3). The remaining process was the same as that of Example 1 to obtain a final magnetic catalytic adsorbent, which was designated as C-3.
[0099] Comparative Example 3
[0100] Weigh 4.3 g of AgNO₃ and dissolve it in 100 ml of deionized water. Then add 10 g of EVS-10 molecular sieves and magnetically stir in a dark environment for 6 hours. Then, filter and rinse repeatedly with deionized water. Dry at 80°C and calcine in a tube furnace at 250°C under a nitrogen atmosphere for 1 hour. This yields a catalytic adsorbent loaded solely with silver nanoparticles, designated Sample D-3.
[0101] The mass fractions of the carrier molecular sieve, active component, magnetic particles in the samples obtained from the above examples and comparative examples, as well as the mass fraction of silicon oxide in the magnetic particles are listed in Table 1.
[0102] Table 1
[0103]
[0104] The mass fraction of manganese oxide is expressed as MnO2.
[0105] Simulated flue gas test example
[0106] The samples synthesized in the above examples and comparative examples were placed in a simulated flue gas experimental system to test the demercuration and denitrification performance. The simulated flue gas conditions are as follows: 5% O2, 12% CO2, 400ppm NO, 400ppm NH3, 600ppm SO2, 30ppm HCl, Hg 0 The concentration is 110 μg / m 3 The balance gas was N2, the total flow rate of the simulated flue gas was 500 mL / min, and the test temperature was 250°C. The flue gas simulation experimental system used can be any conventional experimental system in the art. The mercury removal and denitrification test results are listed in Table 2 below.
[0107] The samples synthesized in the examples and comparative examples were mixed with fly ash, and the separation performance was tested using a magnet. The catalytic adsorbent recovery rates are listed in Table 2 below.
[0108] Table 2
[0109]
[0110]
[0111] According to the data in Table 2 above, it can be seen from the comparison between Example 1 and Comparative Example 1 that the Hg content of the catalyst prepared by using EVS-10 molecular sieve in Example 1 is less than that of the commercially available ETS-10 molecular sieve used in Comparative Example 1. 0 Removal efficiency and NO x The removal efficiency is better.
[0112] Comparing Example 1 with Comparative Example 2, it can be seen that although the product in Comparative Example 2 can also achieve a 100% recovery rate, its mercury removal and denitrification efficiency is much lower than that of Example 1. This shows that the catalytic adsorbent prepared by the method provided in Example 1 using the method provided in the present disclosure has better synergistic mercury removal and denitrification performance on the basis of 100% recovery.
[0113] Comparing Examples 1 to 3 of the present application with Comparative Example 3 (molecular sieve loaded silver), the catalytic adsorbent samples prepared in Examples 1 to 3 can simultaneously remove Hg 0 and NO x And it can achieve a 100% recovery efficiency. However, the nitrogen oxide removal efficiency of the adsorbent obtained in Comparative Example 3 is extremely low, only 21%, and it cannot be recovered by magnets. This shows that the catalytic adsorbent prepared by the method provided by the present disclosure has better synergistic demercuration and denitrification performance and recovery performance.
[0114] Further comparison of Examples 1 to 3 shows that when the dispersion aid is added in Examples 1 to 2, the obtained catalytic adsorbent has a higher Hg 0 Removal efficiency and NO x Removal efficiency.
[0115] The preferred embodiments of the present disclosure are described in detail above. However, the present disclosure is not limited to the specific details of the above embodiments. Within the technical concept of the present disclosure, various simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the scope of protection of the present disclosure. For example,
[0116] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0117] In addition, the various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A magnetic catalytic adsorbent for flue gas demercuration and denitrification, characterized in that: The magnetic catalytic adsorbent comprises a carrier, magnetic particles and an active component; the magnetic particles comprise nano Fe3O4 particles and a silicon oxide layer coated on the surface of the nano Fe3O4 particles, and the active component is loaded on the carrier; the carrier comprises EVS-10 molecular sieve, and the active component comprises manganese oxide; The magnetic catalytic adsorbent is prepared by a method comprising the following steps: (1) mixing magnetic EVS-10 molecular sieve, a manganese source and water to obtain a raw material mixture; (2) adding an alkaline solution and hydrogen peroxide to the raw material mixture to carry out an oxidation reaction; Wherein the magnetic EVS-10 molecular sieve comprises the EVS-10 molecular sieve and the magnetic particles; The raw material mixture in step (1) further comprises a dispersing aid; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride.
2. The catalytic adsorbent according to claim 1, characterized in that: Based on the total weight of the catalytic adsorbent, the mass fraction of the magnetic particles is 5-50% by weight, the mass fraction of the carrier is 35-94% by weight, and the mass fraction of the active component is 1-15% by weight.
3. The catalytic adsorbent according to claim 1, characterized in that: The method further comprises preparing the magnetic EVS-10 molecular sieve by the following steps: a. mixing Fe3O4 particles, a silicate solution and water, and then adding an acid to adjust the pH to obtain a first mixture; b. heating and cooling the first mixture, and then performing a first separation to obtain a first solid product having magnetic properties; c. Dispersing the EVS-10 molecular sieve and the first solid product in a solvent, performing a second separation to remove the solvent; and performing a calcination treatment to obtain the magnetic EVS-10 molecular sieve.
4. The catalytic adsorbent according to claim 3, characterized in that: Step a comprises: adding acid to adjust the pH to 9.3-9.7 to obtain the first mixture.
5. The catalytic adsorbent according to claim 3, characterized in that: In step a, the weight ratio of the Fe3O4 particles, silicate and water is (0.4-1):1:(26-60).
6. The catalytic adsorbent according to claim 5, characterized in that: The silicate comprises sodium silicate; the acid is hydrochloric acid or sulfuric acid; Step a comprises: dispersing the suspension of the Fe3O4 particles and deionized water under ultrasonic treatment and / or mechanical stirring conditions, and then adding the silicate solution.
7. The catalytic adsorbent according to claim 6, characterized in that: The concentration of the silicate solution is 0.5-3 mol / L; the concentration of the acid is 0.1-1 mol / L.
8. The catalytic adsorbent according to claim 3, characterized in that: Step b includes: The first mixture is kept at 30-45°C for 2-4 hours; then the temperature is raised to 85-95°C and kept for 1-2 hours; then the mixture is cooled to 20-40°C.
9. The catalytic adsorbent according to claim 3, characterized in that: In step b, the first separation is performed using a magnetic separation device.
10. The catalytic adsorbent according to claim 3, characterized in that: In step c, the solvent is selected from one or more of toluene, acetone and ethyl acetate.
11. The catalytic adsorbent according to claim 10, characterized in that: The solvent is toluene.
12. The catalytic adsorbent according to claim 3, characterized in that: Step c also includes: adding the carrier molecular sieve to the solvent and mixing with ultrasound, then adding the first solid product and continuing to mix with ultrasound; then standing the obtained suspension to separate layers, removing the upper layer solvent, and then removing the residual solvent under vacuum; In step c, the conditions of the calcination treatment include: a calcination temperature of 250-350° C. and a calcination time of 1-2 hours.
13. The catalytic adsorbent according to claim 1, characterized in that: In step (1), the weight ratio of the magnetic EVS-10 molecular sieve, the manganese source and water is (0.015-0.1): (0.2-0.3): 1; The manganese source is a water-soluble manganese salt.
14. The catalytic adsorbent according to claim 13, characterized in that: The manganese source is selected from one or more of manganese acetate, manganese chloride and manganese nitrate.
15. The catalytic adsorbent according to claim 1, characterized in that: In step (1), the dispersing aid is polymethacrylic acid; Step (1) also includes: mixing the manganese source, water and the dispersing aid, performing ultrasonic treatment and adding the magnetic EVS-10 molecular sieve to obtain the raw material mixture.
16. The catalytic adsorbent according to claim 15, characterized in that: The weight ratio of the dispersing aid to the manganese source is (0.7-3): (2-6).
17. The catalytic adsorbent according to claim 1, characterized in that: In step (2), the alkaline solution is a sodium hydroxide solution; the volume ratio of the sodium hydroxide solution to the water in step (1) is 0.3-0.7:1; The oxidant is hydrogen peroxide, and the concentration of the hydrogen peroxide is 25-35% by weight.
18. The catalytic adsorbent according to claim 1, characterized in that: In step (2), the conditions of the oxidation reaction include: reaction temperature of 40-80°C, reaction time of 0.5-2h; Step (2) also includes: filtering, washing, drying, and then screening the oxidation reaction product; wherein the drying temperature of the oxidation reaction product is 70-110°C.
19. Use of the magnetic catalytic adsorbent according to any one of claims 1 to 18 in the field of flue gas demercurization and denitrification.
20. The use according to claim 19, characterized in that The flue gas is flue gas from a coal-fired power plant.