Amorphous MoS x Nanodisc and its preparation method and use
The amorphous MoS2 nanodisk was prepared by one-step hydrothermal method, which solved the problem of uneven signal of molybdenum disulfide 2H phase, achieved high sensitivity detection of R6G and MB, and demonstrated the excellent performance of amorphous MoSx nanodisk in SERS detection. .
Patent Information
- Application Number
- CN202310079366.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-08
AI Technical Summary
In the prior art, the 2H phase of molybdenum disulfide (MoS2) has a problem of uneven signal signal, resulting in insufficient sensitivity and accuracy of SERS detection, and the synthesis of amorphous MoS2 nanodisks and their SERS performance research has not been reported.
Amorphous MoS2 nanodisks were prepared by one-step hydrothermal method, and highly sensitive SERS detection was achieved through the amorphous structure of the MoS2 nanodisk. The specific steps include dissolving (NH4)2MoS4 in N-N dimethylformamide, and deoxygenation through nitrogen and oxygen. Hydrothermal reaction was carried out, followed by centrifugal decomposition and ultrasonic uniform dispersion, and finally amorphous MoSx nanodisk was obtained and used as a SERS substrate for detection.
High sensitivity detection of R6G and MB dye molecules is achieved, with detection limits reaching 9.23×10-11M and 8.91×10-10M, and enhancement factors reaching 1.67×107 and 6.44×106 respectively, with good SERS performance and comparison Wide linear detection range proves that amorphous MoSx nanodisks have excellent non-precious metal SERS substrate performance.
Smart Images

Figure CN116062793B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an amorphous MoS x The invention discloses a nano disk and a preparation method and application thereof, belonging to the technical field of two-dimensional transition metal sulfide SERS sensing detection. Background Art
[0002] Surface enhanced Raman scattering (SERS) technology has attracted extensive attention from researchers due to its advantages such as convenient operation, high sensitivity, fast detection speed and good reproducibility. Traditional precious metal SERS materials are expensive, so the preparation of low-cost SERS substrates with good signals is the future development direction of SERS technology. In recent years, two-dimensional (2D) layered transition metal sulfides (TMDs) have attracted much attention due to their excellent performance in many application fields such as electronic sensors, energy storage, and catalysis. Molybdenum disulfide (MoS2) has become one of the hot research materials because of its direct band gap and high carrier mobility, as well as some unique properties (such as electrocatalytic hydrogen production, surface enhanced Raman scattering (SERS) characteristics, etc.). The SERS performance of MoS2 is closely related to its phase state. Different phases of MoS2 show different SERS performance. The SERS performance of the metallic 1T phase is better than that of the semiconductor 2H phase. So far, the synthesis of amorphous MoS2 nanodisks and the study of their SERS performance have not been reported. Summary of the invention
[0003] In view of the problem of uneven signal of semiconductor 2H-MoS2, the present invention adopts a one-step hydrothermal method to prepare amorphous MoS2 nanodisks with a higher detection limit, and realizes highly sensitive SERS detection through the amorphous structure of MoS2 nanodisks.
[0004] The present invention is achieved through the following technical solutions:
[0005] An amorphous MoS x Nanodisk, where 1<x≤2.
[0006] An amorphous MoS as described above x A method for preparing a nanodisk comprises the following steps:
[0007] S1. Dissolve (NH4)2MoS4 in NN dimethylformamide, pass nitrogen to remove oxygen, add hydrazine hydrate, and perform hydrothermal reaction at 180-220°C to obtain a primary product;
[0008] S2, after the primary product is centrifuged to remove impurities, the precipitate is collected, ultrasonically dispersed in ultrapure water, and then centrifuged to remove impurities, and the cycle operation is repeated at least 5 times to obtain a crude product;
[0009] S3, adding the crude product into ultrapure water, centrifuging, collecting the supernatant, and obtaining amorphous MoS x Nanodiscs were stored at 4°C.
[0010] As a preferred embodiment, the rotation speed of the centrifugal separation in step S2 is 8000 rpm.
[0011] As a preferred embodiment, the rotation speed of the centrifugal separation in step S3 is 3000 rpm.
[0012] An amorphous MoS as described above x Use of nanodisks in SERS substrates.
[0013] A method for preparing the SERS substrate as described above comprises the following steps:
[0014] Making silicon wafer substrate;
[0015] The amorphous MoS x After the nano-disks are uniformly dispersed by ultrasonication, they are dropped onto the surface of the silicon wafer substrate and allowed to dry naturally at room temperature.
[0016] As a preferred embodiment, the method for preparing the silicon wafer substrate is:
[0017] Take a clean silicon wafer, cut it into 1cm*1cm size, put it into a test tube filled with acetone for ultrasonic cleaning, then use ultrapure water for ultrasonic cleaning, take it out and blow dry it with nitrogen for later use;
[0018] Set the oil bath to 120°C, put the mixed solution into the flask, and when the temperature in the flask is consistent with that of the oil bath, put in the dried silicon wafer, boil at 120°C for 30 minutes, take out and wash with ultrapure water 5 to 6 times, and take out for use.
[0019] As a preferred embodiment, the mixed solution is prepared from concentrated sulfuric acid and hydrogen peroxide in a mass ratio of 3:1.
[0020] The amorphous MoS in the present invention x Nanodisks have good size control and amorphous state, are inexpensive compared to traditional precious metal nanomaterials, and have good biocompatibility. x The nanodisks have semiconductor properties and can further enhance the SERS signal of the dye molecules through a chemical enhancement mechanism.
[0021] Amorphous MoS prepared by the present invention x The nanodisks are uniform in size, ranging from 50 to 80 nm, and are mainly amorphous MoS xThe nanodisks were used as substrates to detect the SERS performance of R6G and MB at different concentrations. The SERS peaks at different points on each substrate were taken. The results showed that for R6G, the detection limit reached 9.23×10 -11 M, the enhancement factor reached 1.67×10 7 For MB, the detection limit reached 8.91×10 -10 M, the enhancement factor reaches 6.44×10 6 , both have good SERS performance, small errors, and a wider linear detection range compared with other substrates.
[0022] In summary, the amorphous MoS prepared by the present invention x The nanodisk exhibits good SERS signal performance and has excellent detection capabilities for two different dye molecules, R6G and MB, and can be used as an efficient non-precious metal SERS substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0024] Figure 1 The amorphous MoS prepared in Example 1 of the present invention x TEM image of nanodisk;
[0025] Figure 2 The single amorphous MoS prepared in Example 1 of the present invention x HRTEM image of nanodisk;
[0026] Figure 3 The single amorphous MoS prepared in Example 1 of the present invention x SAED pattern of nanodisk;
[0027] Figure 4 The single amorphous MoS prepared in Example 1 of the present invention x Mapping diagram of nano disk;
[0028] Figure 5 The amorphous MoS prepared in Example 1 of the present invention x High-resolution Mo3dXPS spectra of nanodisks;
[0029] Figure 6 The amorphous MoS prepared in Example 1 of the present invention x High-resolution S2pXPS spectra of nanodisks;
[0030] Figure 7 The amorphous MoS prepared in Example 1 of the present invention xXPS full spectrum characterization of nanodisks;
[0031] Figure 8 The amorphous MoS prepared in Example 1 of the present invention x XRD characterization of nanodisks;
[0032] Fig. 9 The amorphous MoS prepared in Example 1 of the present invention x EDS spectrum of nanodisk;
[0033] Fig.10 The amorphous MoS prepared in Example 1 of the present invention x Raman detection spectra of the nanodisk substrate for different concentrations of R6G;
[0034] Fig.11 The amorphous MoS prepared in Example 1 of the present invention x Raman spectra of 30 different points of R6G detected on the substrate of the nanodisk;
[0035] Fig.12 The amorphous MoS prepared in Example 1 of the present invention x 1362 cm on the substrate of the nanodisk -1 The log-linear relationship between the peak intensity at and the concentration of R6G molecules;
[0036] Fig.13 The amorphous MoS prepared in Example 1 of the present invention x Average Raman signal intensity map of 30 test points of R6G on the substrate of nanodisk;
[0037] Fig.14 The amorphous MoS prepared in Example 1 of the present invention x Raman detection spectra of the nanodisk substrate for different concentrations of MB;
[0038] Fig.15 The amorphous MoS prepared in Example 1 of the present invention x Raman spectra of 30 different points on the substrate of the nanodisk where MB was detected;
[0039] Fig.16 The amorphous MoS prepared in Example 1 of the present invention x 1626 cm on the substrate of nanodisk -1 The log-linear relationship between the peak intensity at and the MB molecular concentration;
[0040] Fig.17 The amorphous MoS prepared in Example 1 of the present invention x Average Raman signal intensity plot of 30 test points of MB on the substrate of nanodisk.
[0041] Fig.18 TEM image of 1T-MoS2 nanoflower prepared in Comparative Example 1 of the present invention;
[0042] Fig.19 HRTEM image of 1T-MoS2 nanoflower prepared in Comparative Example 1 of the present invention;
[0043] Fig. 20 This is a high-resolution transmission electron microscopy image of the 1T-MoS2 nanoflower prepared in Comparative Example 2 of the present invention;
[0044] Fig.21 This is a scanning electron microscope image of the 1T-MoS2 nanoflower prepared in Comparative Example 2 of the present invention;
[0045] Fig. 22 This is the XRD characterization diagram of the 1T-MoS2 nanoflower prepared in Comparative Example 2 of the present invention;
[0046] Fig.23 This is a Raman spectrum characterization diagram of the 1T-MoS2 nanoflower prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0047] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0048] The raw materials in the present invention are all commercially available.
[0049] Among them, (NH4)2MoS4 and hydrazine hydrate were purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd. NN dimethylformamide was purchased from Shanghai MacLean Co., Ltd.
[0050] Example 1
[0051] This embodiment provides an amorphous MoS x The preparation method of the nanodisk specifically comprises the following steps:
[0052] First, weigh 2.6 mg of (NH4)2MoS4, put it into a glass bottle with a volume of about 20 mL, add 10 mL of NN dimethylformamide solution, put it into an ultrasonic machine for 15 minutes to obtain a clear and uniform solution, and continue to pass nitrogen for 30 minutes for deoxygenation. The mixed solution was transferred into a 20 mL stainless steel high-pressure reactor lined with tetrafluoroethylene, and then 100 μL of hydrazine hydrate was added. It was placed in an oven, the temperature was set to 200 ° C, and the reaction was 30 minutes. After cooling to room temperature, it was taken out. The initial product was centrifuged to remove impurities, the separation speed was 8000 rpm, and the time was 10 minutes. The precipitate was collected and ultrasonically dispersed uniformly in ultrapure water, and the above purification steps were repeated 5 times. 5 mL of ultrapure water was added to the last precipitate, and the larger size products were removed by low-speed centrifugation. The speed was 3000 rpm, and the time was 8 minutes. The supernatant was collected to obtain amorphous MoS x The nanoplates were stored in a 4°C refrigerator.
[0053] The amorphous MoS prepared in Example 1 x The nanodisks were characterized by TEM images ( Figure 1 ) Observe the obtained amorphous MoS x The nanodisks are disc-shaped, evenly dispersed, and have an average particle size of about 50-80 nm. HRTEM analysis of amorphous MoS x The structure of the nanodisk ( Figure 2 ), it can be seen that there is no obvious lattice fringes. HRTEM characterization preliminarily proves that amorphous MoS x The amorphous structure of the nanodisk. Selected area electron diffraction (SAED) shows that there are no obvious diffraction spots ( Figure 3 ). HRTEM and SAED preliminarily proved its amorphous structure. By mapping the material ( Figure 4 ) and EDS spectrum ( Fig. 9 ) calculation, the ratio of Mo and S is 1:2, confirming that the material is amorphous MoS x Nanodisks. Amorphous MoS x The atomic valence states in the nanodisks were determined by X-ray photoelectron spectroscopy (XPS), e.g. Figure 5 , 6 As shown, the XPS spectrum peaks of Mo3d are located at 229.3eV and 232.5eV, corresponding to the Mo3d of zero-valent Mo, respectively. 5 / 2 and Mo3d 3 / 2 The XPS spectrum peaks of S2p are located at 162.0eV and 163.3eV, respectively, which are attributed to the S2p of zero-valent S. 3 / 2 and S2p 5 / 2 . Figure 7 The amorphous MoS prepared in Example 1 xXPS full spectrum characterization of nanodisks. Figure 8 The amorphous MoS prepared in Example 1 x The XRD characterization diagram of the nanodisk shows that amorphous MoS x Compared with the clean silicon substrate, the nanodisk has no obvious crystallinity. TEM, HRTEM, EDS calculation and XPS characterization further prove that the amorphous MoS x Successful synthesis of nanodisks with x=2.
[0054] The amorphous MoS prepared in Example 1 x Nanodisks are used for substrate fabrication.
[0055] First, make a silicon wafer substrate. Take a clean silicon wafer and cut it into 1cm*1cm size. Put it into a test tube filled with acetone and ultrasonically clean it for 30 minutes. Then, use ultrapure water to ultrasonically clean it for 30 minutes. Take it out and blow it dry with nitrogen for later use. Set the oil bath to 120℃, put a mixed solution (concentrated sulfuric acid: hydrogen peroxide = 3:1) in the flask, and when the temperature in the flask is consistent with the temperature of the oil bath, put the dried silicon wafer in, boil it at 120℃ for 30 minutes, then take it out and wash it with ultrapure water for 5 to 6 times, and put it away for later use. The amorphous MoS prepared in Example 1 x The nanodisk was ultrasonically homogenized, and 40 μL of the solution was dropped on a silicon wafer (the silicon wafer should be dried with nitrogen again before use), and then naturally dried at room temperature to obtain amorphous MoS x Nanodisk substrate. Then, two dye molecular solutions of rhodamine 6G (R6G) and methyl blue (MB) with different concentrations were prepared, with a concentration gradient of 10 -3 M~10 -12 M, put the fully dried substrate into the dye solution with the material side facing up, take it out after soaking overnight, rinse the free dye molecules on the surface of the substrate with deionized water, blow it dry with nitrogen, and then prepare for Raman testing.
[0056] The amorphous MoS prepared above x The SERS signal of the nanodisk substrate was detected. When testing the substrate immersed in the R6G solution, the Raman test conditions were set to 532nm and the scanning wave number range was 800-2000cm -1 , 30 test points were selected on each substrate, the test power was 0.1mW, and the exposure time was 5s. Fig.10 Amorphous MoS x Raman detection spectra of the nanodisk substrate for different concentrations of R6G, 1362 cm -1 Obvious Raman characteristic peaks can be seen at the bottom. And for different concentrations of R6G, the peak intensity is different. As the concentration of R6G decreases, the Raman characteristic peak gradually weakens. It is concluded that the linear detection range for R6G is 10 -10M~10 -4 M, the detection limit was calculated to be 9.23×10 -11 M, the enhancement factor reached 1.67×10 7 ; Fig.11 These are the Raman spectra of 30 different points on the substrate, from which the uniformity of the Raman signal can be seen. Fig.12 Amorphous MoS x 1362 cm on nanodisk substrate -1 The logarithmic linear relationship between the peak intensity at 1362 cm and the concentration of R6G dye molecules is shown in the figure. -1 The Raman peak at shows a good linear relationship with the concentration of R6G. Fig.13 Amorphous MoS x The average Raman signal intensity of 30 test points on the nanodisk substrate shows that the average intensity of the Raman signal is 3989.15, and the relative error is 4.91%. It can be seen that the signal uniformity of the substrate is good and the error is small.
[0057] When testing the substrate immersed in MB solution, the Raman test conditions were modified to a wavelength of 785 nm, while other conditions remained unchanged. Fig.14 Amorphous MoS x Raman detection spectra of the nanodisk substrate for different MB concentrations, where 1626 cm -1 Obvious Raman characteristic peaks can be seen at the bottom. And for different concentrations of MB, the peak intensity is different. As the concentration of MB decreases, the Raman characteristic peak gradually weakens. It is concluded that the linear detection range for MB is 10 -9 M~10 -4 M, the detection limit was calculated to be 8.91×10 -10 M, the enhancement factor reaches 6.44×10 6 ; Fig.15 It is the Raman spectrum of 30 different points on the substrate, and the uniformity of the Raman signal can be seen. Fig.16 Amorphous MoS x 1626 cm on nanodisk substrate -1 The logarithmic linear relationship between the peak intensity at 1626 cm and the concentration of MB dye molecules is shown in the figure. -1 The Raman peak at shows a good linear relationship with the concentration of MB. Fig.17 Amorphous MoS x The average Raman signal intensity of 30 test points on the nanodisk substrate shows that the average intensity of the Raman signal is 3605.11, with a relative error of 5.27%. It can be seen that the substrate also has good signal uniformity and a small error range. The Raman detection of the two dye molecules has a lower detection limit and good signal uniformity, which also shows that the synthesized amorphous MoSx The nanodisks have good SERS substrate properties.
[0058] Comparative Example 1
[0059] The method of this comparative example is basically the same as that of Example 1, except that the time duration in the hydrothermal reaction condition is extended to 12 h and the reaction temperature is increased to 200° C. to obtain 1T-MoS2 nanoflowers instead of nanodisks.
[0060] The 1T-MoS2 nanoflowers prepared in Comparative Example 1 were characterized. From the TEM image ( Fig.18 ) The obtained product is observed to be in the shape of nanoflowers, evenly dispersed, and with clear particles. The structure of 1T-MoS2 nanoflowers was analyzed by HRTEM ( Fig.19 ), we can see obvious lattice fringes, and HRTEM characterization proves that 1T-MoS2 nanoflowers have a lattice structure. HRTEM of 1T-MoS2 nanoflowers proves that 1T-MoS2 nanoflowers are different from amorphous MoS x Differences in structure between nanodisks: amorphous MoS x The nanodisks are disc-shaped, evenly dispersed, without obvious lattice fringes, and the average particle size is about 50-80nm, while the 1T-MoS2 nanoflowers are scattered in a flower-like shape, and clear lattice fringes can be seen, indicating that a longer reaction time will not produce amorphous MoS x .
[0061] Comparative Example 2
[0062] This comparative example provides a method for preparing a metallic phase MoS2-CoNi(OH)2 nanocomposite material, which specifically comprises the following steps:
[0063] 2.6 mg (NH4)2MoS4 was added to 10 mL DMF and ultrasonicated for 10 min to obtain a clear and homogeneous (NH4)2MoS4 solution;
[0064] Take 10mL (NH4)2MoS4 solution and 100μL hydrazine hydrate, mix them into a reaction solution and add them into a 20mL hydrothermal kettle lined with Teflon coating, then immerse a carbon paper with a length of 2.5cm and a width of 0.25cm in the reaction solution, heat the hydrothermal kettle at 200℃ for 12 hours to obtain a carbon paper with a metallic phase MoS2 grown on it, wash it with deionized water and set it aside;
[0065] The carbon paper grown with the metallic phase MoS2 was used as a working electrode and immersed in a 10 mL electrolyte solution (the solvent was water) containing 1.5 mM Co(NO3)3 and 1.5 mM Ni(NO3)3. A platinum wire was used as a counter electrode and a saturated calomel electrode was used as a reference electrode. CoNi(OH)2 nanosheets were deposited on the surface of the carbon paper grown with the metallic phase MoS2 by constant potential electrodeposition at -1.0 V (vs. SCE) for 300 s to obtain a metallic phase MoS2-CoNi(OH)2 nanocomposite material.
[0066] The carbon paper with metallic phase MoS2 prepared in this comparative example was characterized, and the results of X-ray energy spectrum analysis and element imaging analysis confirmed the presence of Mo and S elements; high-resolution transmission electron microscopy photos are shown in FIG. Fig. 20 As shown in Figure 2, a typical MoS2 interlayer spacing (0.635 nm) appeared, confirming the successful formation of MoS2 nanosheets on carbon paper; scanning electron microscope photos are shown in Figure 2 Fig.21 As shown in Figure 2, thin layers of MoS2 are grown on carbon paper. X-ray diffraction images are shown in Figure 2. Fig. 22 As shown, the XRD peak at 9.0° is attributed to the (002) plane of MoS2 into which oxygen is introduced due to the formation of a layered structure, the diffraction peak at 18.0° is attributed to the (004) plane of MoS2, and the diffraction peaks at 32.2° and 56.7° correspond to the (100) and (110) crystal planes of MoS2. The broad diffraction peaks of (100) and (110) indicate the weak crystallinity of the prepared MoS2. The structure and composition of the prepared MoS2 were characterized by Raman spectroscopy, as shown in Figure 1. Fig.23 As shown, 144(J1)cm -1 , 219(J2)cm -1 and 247(J3)cm -1 It is a typical Raman peak of metallic phase MoS2 at 289cm -1 E 1g The vibration mode is generated by the metallic octahedral coordinated MoS2, 193 cm -1 The Raman peaks at 371 cm -1 and 401cm -1 The two peaks at correspond to the E 2g 1 and A 1g mode, Raman characterization confirmed the coexistence of 1T and 2H phases in the product, and XPS analysis showed that the product was mainly metallic phase.
[0067] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. Amorphous MoS x Preparation method of nanodisks, It is characterized in that The steps include: S1, 2.6 mg (NH 4 ) 2 MoS 4 Dissolve in N-N dimethylformamide, pass nitrogen to remove oxygen, add 100 μL of hydrazine hydrate, and perform hydrothermal reaction at 200 °C for 30 min to obtain the initial product; S2, after the primary product is centrifuged to remove impurities, the precipitate is collected, ultrasonically dispersed in ultrapure water, and then centrifuged to remove impurities, and the cycle operation is repeated at least 5 times to obtain a crude product; S3, adding the crude product into ultrapure water, centrifuging, collecting the supernatant, and obtaining amorphous MoS x Nanodiscs were stored at 4 °C; The amorphous MoS x Nanodisks are disc-shaped with an average particle size of 50-80 nm, where x=2.
2. The amorphous MoS according to claim 1 x Preparation method of nanodisks, It is characterized in that The rotation speed of the centrifugal separation in step S2 is 8000 rpm.
3. The amorphous MoS according to claim 1 x Preparation method of nanodisks, It is characterized in that The rotation speed of the centrifugal separation in step S3 is 3000 rpm.
4. Amorphous MoS obtained by the preparation method according to any one of claims 1 to 3 x Use of nanodisks in SERS substrates.
5. The amorphous MoS according to claim 4 x Use of nanodisks in SERS substrates, It is characterized in that The preparation method of the SERS substrate comprises the following steps: Making silicon wafer substrate; The amorphous MoS x After the nano-disks are uniformly dispersed by ultrasonication, they are dropped onto the surface of the silicon wafer substrate and allowed to dry naturally at room temperature.
6. Use of the amorphous MoSx nanodisk as claimed in claim 5 in a SERS substrate, It is characterized in that The preparation method of the silicon wafer substrate is as follows: Take a clean silicon wafer, cut it into 1 cm * 1 cm size, put it into a test tube filled with acetone for ultrasonic cleaning, then use ultrapure water for ultrasonic cleaning, take it out and blow dry it with nitrogen for later use; Set the oil bath to 120 ℃, put the mixed solution into the flask, and when the temperature in the flask is consistent with that of the oil bath, put in the dried silicon wafer, boil at 120 ℃ for 30 min, take out and wash with ultrapure water 5 to 6 times, and take out for use.
7. Use of the amorphous MoSx nanodisk as claimed in claim 6 in a SERS substrate, It is characterized in that The mixed solution is prepared from concentrated sulfuric acid and hydrogen peroxide in a mass ratio of 3:1.