Compounds and their use as binders in carbon-coated copper foil

By using the binder of benzotriazole and silane coupling agent in the carbon-copper foil coated with lithium-ion batteries, the problems of high internal resistance and low adhesion in the prior art are solved, and low resistance is achieved Combined with high bonding forces, it improves water resistance and solvent resistance.

CN116063343BActive Publication Date: 2024-11-08DONGGUAN DONGYANG SOLAR SCI RES & DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310024395.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-11-08
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

The existing lithium-ion battery-coated carbon-copper foil is difficult to meet the requirements of low internal resistance and high adhesion when improving the adhesion, and it has poor water resistance and solvent resistance.

Method used

Using a binder containing benzotriazole and silane coupling agent, a covalent bond and coordination bond are formed with the copper atom by benzotriazole, and alkoxy-coupled conductive filler in the silane coupling agent. Improve the bonding force between the copper foil and the coating and the bonding force of the conductive filler, and enhance the corrosion resistance of the copper foil.

Benefits of technology

In the case of low usage, low resistance and high adhesion of carbon-coated copper foil are achieved, the comprehensive performance of carbon-coated copper foil is improved, and its water resistance and solvent resistance are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116063343B_ABST
    Figure CN116063343B_ABST
Patent Text Reader

Abstract

The present invention provides a compound and its application as a binder in carbon-coated copper foil for lithium-ion batteries. The structural formula of the compound is shown in formula (I), wherein R 1 and R 2 The compound has the meaning described in the specification. The compound has good adhesion under the condition of small dosage. The carbon-coated copper foil prepared by using the compound as a binder has both low resistance and strong adhesion, which improves the comprehensive performance of the carbon-coated copper foil. In addition, since the benzotriazole structure has a certain passivation effect on the copper foil, it can also improve the corrosion resistance of the copper foil, thereby improving the water resistance and solvent resistance of the carbon-coated copper foil. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of batteries, in particular to a compound and application thereof in carbon-coated copper foil of lithium ion batteries. Background Art

[0002] Lithium-ion batteries have the characteristics of high voltage, high energy density, long cycle life, no memory effect, and are green, environmentally friendly, safe, reliable, and fast charging and discharging. They have attracted the attention and extensive research of the country, enterprises, and more and more scholars. Carbon coating of copper foil is a common method to improve the performance of lithium iron phosphate batteries, but the bonding force of commonly used carbon coating slurries is low. If the amount of binder is increased to improve the bonding force, the internal resistance of the carbon-coated copper foil will increase. That is, the formula of ordinary carbon coating slurry cannot meet the requirements of low internal resistance and high bonding force at the same time. In addition, the carbon-coated copper foil prepared by commonly used carbon coating slurries also has the problem of poor water resistance and solvent resistance.

[0003] CN102498600A discloses a copper foil for a collector of a lithium ion battery, and the copper foil is surface treated by a mixed solution of a silane coupling agent and an azole surface treatment agent at one time, so that the adhesion obtained by the surface treatment of the silane coupling agent and the rust resistance obtained by the surface treatment of the azole compound can be taken into account. The patent uses a mixture of a silane coupling agent and an azole compound, and then uses the adhesion of the silane coupling agent and the rust resistance of the azole compound. The two are coordinated to improve the adhesion and rust resistance of the copper foil in a balanced manner, and it is necessary to detect and analyze the mixed layer formed by the mixed solution for surface treatment to determine whether a mixed layer formed by the mixed solution of the silane coupling agent and the azole surface treatment agent is formed, rather than forming a separate layer generated by silane coupling or azole compounds. In the case where the surface treatment using the silane coupling agent and the surface treatment using the azole surface treatment agent are performed separately and superimposed (overlapping coating of the surface treatment agent), this effect cannot be obtained. The process of this patent is complicated, and the adhesion is improved only by using a silane coupling agent. There is no report on improving the adhesion of the copper foil while satisfying the characteristic of low internal resistance.

[0004] Therefore, the problems existing in the above-mentioned existing carbon-coated copper foil, especially the adhesion problem, need to be improved urgently. Summary of the invention

[0005] The purpose of the present invention is to provide a compound and its use as a binder in carbon-coated copper foil for lithium ion batteries in view of the deficiencies in the prior art. The compound has good bonding strength under the condition of small dosage. The carbon-coated copper foil prepared by using the compound as a binder has both low resistance and strong bonding strength, thereby improving the comprehensive performance of the carbon-coated copper foil. In addition, since the benzotriazole functional group has a certain passivation effect on the copper foil, the corrosion resistance of the copper foil can also be improved, thereby improving the water resistance and solvent resistance of the carbon-coated copper foil.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] In a first aspect, the present invention provides a compound, wherein the compound is a compound as represented by formula (I) or a stereoisomer or tautomer of the compound as represented by formula (I),

[0008]

[0009] in:

[0010] R1 is C 1-4 Alkyl, R2 is C 1-6 Alkylene.

[0011] Preferably, R1 is methyl, ethyl, n-propyl, isopropyl, n-butyl or isobutyl; R2 is methylene, 1,2-ethylene, 1,3-propylene, 2-methyl-1,3-propylene, 1,4-butylene, 2,2-dimethyl-1,4-butylene.

[0012] Preferably, the compound has one of the following structures or a stereoisomer or tautomer having one of the following structures:

[0013]

[0014] The synthesis method of the compound is as follows:

[0015]

[0016] Wherein, R1 and R2 in compound A have the meanings described in the present invention.

[0017] (1) Synthesis of 1,2,3-benzotriazole-5-carboxylic acid methyl ester

[0018] 7.3 g (0.044 mol) of methyl 3,4-diaminobenzoate was dissolved in 100 mL of acetic acid, and 3.36 g (0.048 mol) of sodium nitrite was slowly added. The mixture was stirred at room temperature for 18 hours. After the reaction was complete, the reaction solution was poured into 300 mL of water, and the pH value was adjusted to neutral with sodium carbonate. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid.

[0019] (2) Synthesis of 5-carboxylic acid benzotriazole

[0020] 8.49 g (0.048 mol) of 1,2,3-benzotriazole-5-carboxylic acid methyl ester was dispersed in 100 mL of water, and 200 mL of sodium hydroxide solution was slowly added. The mixture was stirred at 40° C. for 4 hours. After the reaction was complete, the mixture was cooled to room temperature, and the pH value was adjusted to neutral with hydrochloric acid. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid.

[0021] (3) Synthesis of 1H-benzothiazole-5-carbonyl chloride

[0022] Dissolve 9.1 g (0.056 mol) of 5-carboxylic acid benzotriazole in 500 mL of dichloromethane, slowly add 20-100 mL of oxalyl chloride, stir at room temperature for 0.5-4 hours, evaporate the solvent under reduced pressure, and dissolve the remaining reaction product in 50-100 mL of dichloromethane to obtain a dichloromethane solution of 1H-benzothiazole-5-carbonyl chloride.

[0023] (4) Synthesis of Compound (I)

[0024] To the above 50-100 mL of dichloromethane mixed solution, add 0.05-0.06 mol of compound A and 0.01-0.03 mol of triethylamine, stir at 20-60° C. for 3-10 hours, evaporate the solvent under reduced pressure, and obtain compound (I) by column chromatography.

[0025] In a second aspect, the present invention provides an adhesive for carbon-coated copper foil, comprising one or more of the compounds described in the present invention.

[0026] The adhesive of the present invention contains a benzotriazole structure at one end and a silane coupling agent structure at the other end. First, the benzotriazole structure can form covalent bonds and coordination bonds with copper atoms, which alternately form chain polymers to increase the bonding force between the adhesive and the copper foil. Second, the alkoxy group in the silane coupling agent structure is used to couple the conductive filler, thereby increasing the bonding force between the adhesive and the conductive filler. Through the special effects of the above two functional groups, the problem of good bonding between the copper foil and the coating layer can be solved in the case of a small amount, and the internal resistance of the carbon-coated copper foil will not be increased. In addition, benzotriazole has a certain passivation effect on the copper foil, which can improve the corrosion resistance of the copper foil, thereby improving the water resistance and solvent resistance of the carbon-coated copper foil.

[0027] In a third aspect, the present invention provides a method for preparing a carbon-coated copper foil, comprising the following steps:

[0028] S1. preparing a carbon coating slurry: adding a dispersant and a dispersing aid into a solvent for dispersion, adding a conductive agent, and finally adding the binder described in claim 4 to obtain a carbon coating slurry;

[0029] S2, coating: taking the above carbon coating slurry and coating it on the copper foil;

[0030] S3, drying: drying the coated copper foil to obtain the carbon-coated copper foil.

[0031] Preferably, in the step S1, based on 100 parts of the total weight of the carbon coating slurry, the binder is 0.5 to 2 parts, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0 parts.

[0032] Preferably, in the step S1, based on the total weight of the carbon-coated slurry as 100 parts, the dispersant is 0.1 to 2 parts, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0 parts; the dispersing aid is 0.1 to 1 part, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 part; the conductive agent is 2 to 18 parts, for example, 2, 6, 10, 14, 18 parts; further preferably, the conductive agent is 4 to 16 parts, for example, 4, 10, 16; further preferably, the conductive agent is 8 to 12 parts, for example, 8, 10, 12; the rest is solvent; wherein the solvent is water.

[0033] Preferably, the dispersant is one or more of BYK22092, BYK440, BYK206, and BYK019; the dispersing aid is one or more of ethanol, n-butanol, tert-butanol, n-propanol, isopropanol, propylene glycol methyl ether, and propylene glycol butyl ether.

[0034] Preferably, the conductive agent is one or more of graphite, carbon black, carbon nanotubes, and graphene.

[0035] The beneficial effects of the present invention are:

[0036] (1) The compound described in formula (1) of the present invention can have good adhesion under the condition of small dosage. Thus, the carbon-coated copper foil prepared by using it as a binder has both low resistance and strong adhesion, thereby improving the comprehensive performance of the carbon-coated copper foil. The mechanism of action is as follows: first, benzotriazole can form covalent bonds and coordination bonds with copper atoms, alternately forming chain polymers, thereby increasing the bonding force between the binder and the copper foil; second, the alkoxy group in the silane coupling agent structure is used to couple the conductive filler, thereby increasing the bonding force between the binder and the conductive filler. Through the special effects of the above-mentioned two structures of benzotriazole and silane coupling agent, the problem of having good adhesion between the copper foil and the coating layer under the condition of small dosage is solved without increasing the internal resistance of the carbon-coated copper foil.

[0037] (2) The carbon-coated copper foil prepared by using the compound described in formula (1) as a binder has good water resistance and solvent resistance. The mechanism of action is that the benzotriazole structure in the binder has a certain passivation effect on the copper foil, which can improve the corrosion resistance of the copper foil, thereby improving the water resistance and solvent resistance of the carbon-coated copper foil.

[0038] Definition of terms

[0039] In the present invention, when the name and structure of a compound conflict, the structure of the compound shall prevail.

[0040] Unless expressly stated to the contrary, all ranges cited herein are inclusive.

[0041] The term "a" or "an" used in the present invention is used to describe the elements and components described in the present invention. This is done only for convenience and to provide a general sense of the scope of the present invention. This description should be understood to include one or at least one, and the singular also includes the plural, unless it is obvious that it is otherwise intended. "Multiple" means two or more.

[0042] The numbers in the present invention are approximate values, regardless of whether the words "about" or "approximately" are used. The numerical values ​​of the numbers may differ by 1%, 2%, 5%, 7%, 8%, 10%, etc. Whenever a number with a value of N is disclosed, any number with a value of N+ / -1%, N+ / -2%, N+ / -3%, N+ / -5%, N+ / -7%, N+ / -8% or N+ / -10% will be explicitly disclosed, where "+ / -" means plus or minus, and the range between N-10% and N+10% is also disclosed.

[0043] Unless otherwise indicated, the following definitions used in the present invention shall apply. For purposes of the present invention, chemical elements are consistent with the Periodic Table of the Elements, CAS version, and the 75th edition of the Handbook of Chemistry and Physics, 1994. In addition, general principles of organic chemistry can be found in "Organic Chemistry", Thomas Sorrell, University Science Books, Sausalito: 1999, and "March's Advanced Organic Chemistry" by Michael B. Smith and Jerry March, John Wiley & Sons, New York: 2007, the entire contents of which are incorporated herein by reference.

[0044] The term “comprise” or “include” is an open expression, that is, including the contents specified in the present invention but not excluding other contents.

[0045] The term "stereoisomers" refers to compounds with the same chemical structure but different arrangements of atoms or groups in space. Stereoisomers include enantiomers, diastereomers, conformers (rotamers), geometric isomers (cis / trans) isomers, and atropisomers, etc.

[0046] The stereochemical definitions and conventions used in the present invention generally follow those described in SP Parker, Ed., McGraw-Hill Dictionary of Chemical Terms (1984) McGraw-Hill Book Company, New York; and Eliel, E. and Wilen, S., "Stereochemistry of Organic Compounds", John Wiley & Sons, Inc., New York, 1994.

[0047] Many organic compounds exist in optically active forms, i.e. they have the ability to rotate the plane of plane polarized light. When describing an optically active compound, the prefixes D and L, or R and S are used to indicate the absolute configuration of the molecule about its chiral center(s). The prefixes d and l, or (+) and (-), are the symbols used to designate the rotation of plane polarized light caused by the compound, where (-) or l indicates that the compound is left-handed. Compounds prefixed with (+) or d are right-handed. A specific stereoisomer is an enantiomer, and a mixture of such isomers is called a mixture of enantiomers. A 50:50 mixture of enantiomers is called a racemic mixture or racemate, which can occur when there is no stereoselectivity or stereospecificity in a chemical reaction or process.

[0048] Any asymmetric atom (e.g., carbon, etc.) of the compounds disclosed herein can exist in a racemic or enantiomerically enriched form, such as in the (R)-, (S)-, or (R,S)-configuration. In certain embodiments, each asymmetric atom has at least 50% enantiomeric excess, at least 60% enantiomeric excess, at least 70% enantiomeric excess, at least 80% enantiomeric excess, at least 90% enantiomeric excess, at least 95% enantiomeric excess, or at least 99% enantiomeric excess in terms of the (R)- or (S)-configuration.

[0049] Depending on the choice of starting materials and process, the compounds of the invention may exist in the form of one of the possible isomers or a mixture thereof, such as a racemate and a diastereomeric mixture (depending on the number of asymmetric carbon atoms). Optically active (R)- or (S)-isomers may be prepared using chiral synthons or chiral reagents, or resolved using conventional techniques. If the compound contains a double bond, the substituents may be in the E or Z configuration; if the compound contains a disubstituted cycloalkyl group, the cycloalkyl substituents may be in the cis or trans configuration.

[0050] Any resulting mixture of stereoisomers can be separated into the pure or substantially pure geometric isomers, enantiomers, diastereomers on the basis of the differences in the constituent physicochemical properties, for example, by chromatography and / or fractional crystallization.

[0051] Any racemate of the final product or intermediate obtained can be separated into optical antipodes by known methods by methods familiar to those skilled in the art, such as by separation of the diastereoisomeric salts obtained thereof. The racemic product can also be separated by chiral chromatography, such as high performance liquid chromatography (HPLC) using a chiral adsorbent. In particular, enantiomers can be prepared by asymmetric synthesis, for example, see Jacques, et al., Enantiomers, Racemates and Resolutions (Wiley Interscience, New York, 1981); Principles of Asymmetric Synthesis (2nd Ed. Robert E. Gawley, Jeffrey Aubé, Elsevier, Oxford, UK, 2012); Eliel, EL Stereochemistry of Carbon Compounds (McGraw-Hill, NY, 1962); Wilen, SH Tables of Resolving Agents and Optical Resolutions p. 268 (EL Eliel, Ed., Univ. of Notre Dame Press, Notre Dame, IN 1972); Chiral Separation Techniques: A Practical Approach (Subramanian, G. Ed., Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim, Germany, 2007).

[0052] The term "tautomer" or "tautomeric form" refers to structural isomers with different energies that can be mutually converted through a low energy barrier. If tautomerism is possible (such as in solution), a chemical equilibrium of tautomers can be reached. For example, proton tautomers (protontautomers) (also known as prototropic tautomers) include mutual conversions by proton migration, such as keto-enol isomerization and imine-enamine isomerization. Valence tautomers include mutual conversions by the reorganization of some bonding electrons. A specific example of keto-enol tautomerism is the interconversion of pentane-2,4-dione and 4-hydroxypent-3-ene-2-one tautomers. Another example of tautomerism is phenol-keto tautomerism. A specific example of phenol-keto tautomerism is the interconversion of pyridine-4-ol and pyridine-4 (1H)-one tautomers. Unless otherwise stated, all tautomeric forms of the compounds of the invention are within the scope of the invention.

[0053] In various parts of this specification, the substituents of the compounds disclosed in the present invention are disclosed according to group types or ranges. It is particularly pointed out that the present invention includes each independent subcombination of the individual members of these group types and ranges. For example, the term "C 1-4 "Alkyl" specifically refers to methyl, ethyl, C3 alkyl and C4 alkyl as disclosed independently.

[0054] The term "alkyl" or "alkyl group" refers to a saturated straight or branched chain hydrocarbon group. In one embodiment, the alkyl group contains 1-4 carbon atoms; in another embodiment, the alkyl group contains 1-3 carbon atoms; in another embodiment, the alkyl group contains 1-2 carbon atoms; in another embodiment, the alkyl group contains 1 carbon atom. Examples of alkyl groups include, but are not limited to, methyl (Me, -CH3), ethyl (Et, -CH2CH3), n-propyl (n-Pr, -CH2CH2CH3), isopropyl (i-Pr, -CH(CH3)2), n-butyl (n-Bu, -CH2CH2CH2CH3), isobutyl (i-Bu, -CH2CH(CH3)2), and the like.

[0055] The term "alkylene" means a saturated divalent hydrocarbon radical obtained by removing two hydrogen atoms from a saturated straight or branched hydrocarbon. In one embodiment, the alkylene group contains 1-6 carbon atoms; in another embodiment, the alkylene group contains 1-4 carbon atoms; in yet another embodiment, the alkylene group contains 1-3 carbon atoms; in yet another embodiment, the alkylene group contains 1-2 carbon atoms. Non-limiting examples include methylene (-CH2-), ethylene (-CH2CH2-), isopropylene (-CH(CH3)CH2-), and the like.

[0056] BYK22092, BYK440, BYK206 and BYK019 are all different types of dispersants produced by BYK Chemical Company of Germany. BYK22092 is an acrylate copolymer ammonium salt solution, BYK440 is a modified polyamide solution, BYK206 is an anionic unsaturated fatty acid alkanolamine salt solution, and BYK019 is a polyether modified polydimethylsiloxane.

[0057] Unless otherwise defined, the meaning of all scientific and technological terms used in the present invention is the same as those of ordinary skill in the art to which the present invention belongs. Although methods and materials similar or equivalent to the methods and materials described in the present invention can also be used in the implementation or testing of embodiments of the present invention, suitable methods and materials are described below. All publications, patent applications, patents and other references mentioned in the present invention are incorporated into the present invention by reference in their entirety, unless specific paragraphs are cited. If a conflict occurs, this specification and the definitions included therein shall prevail. In addition, materials, methods and embodiments are only illustrative and are not intended to be limiting. DETAILED DESCRIPTION

[0058] The following description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0059] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0060] In the examples described below, unless otherwise specified, all temperatures are in degrees Celsius. The reagents used can be purchased from the market or prepared by the methods described in the present invention.

[0061] In the present invention, if there is any discrepancy between the chemical name and the chemical structure, the structure prevails.

[0062] The following abbreviations are used throughout this document:

[0063] g grams

[0064] mL ml

[0065] mol

[0066] m m

[0067] mm mm

[0068] μm micrometer

[0069] h hours

[0070] min

[0071] s seconds

[0072] r / min

[0073] ℃ Celsius

[0074] wt%

[0075] mΩ / □milliohm / square

[0076] Ω / □Ohm / square

[0077] N Newton

[0078] Example 1 Synthesis of Compound B1

[0079]

[0080] 7.3 g (0.044 mol) of methyl 3,4-diaminobenzoate was dissolved in 100 mL of acetic acid, and 3.36 g (0.048 mol) of sodium nitrite was slowly added. The mixture was stirred at room temperature for 18 hours. After the reaction was complete, the reaction solution was poured into 300 mL of water, and the pH value was adjusted to neutral with sodium carbonate. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid with a yield of 77%.

[0081] 8.49 g (0.048 mol) of 1,2,3-benzotriazole-5-carboxylic acid methyl ester was dispersed in 100 mL of water, and 200 mL of sodium hydroxide solution was slowly added. The mixture was stirred at 40°C for 4 hours. After the reaction was complete, the mixture was cooled to room temperature, and the pH value was adjusted to neutral with hydrochloric acid. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid. The yield was 67%.

[0082] 9.1 g (0.056 mol) of 5-carboxylic acid benzotriazole was dissolved in 500 mL of dichloromethane, 20 mL of oxalyl chloride was slowly added, and the mixture was stirred at room temperature for 0.5 hour. The solvent was evaporated under reduced pressure, and the remaining reaction product was dissolved in 50 mL of dichloromethane to obtain a dichloromethane solution of 1H-benzothiazole-5-carbonyl chloride.

[0083] To the above 50 mL of dichloromethane mixed solution, 8.96 g (0.05 mol) of 3-aminopropyltrimethoxysilane and 1.01 g (0.01 mol) of triethylamine were added, and the mixture was stirred at 20° C. for 10 hours. The solvent was evaporated under reduced pressure, and compound B1 was obtained by column chromatography with a yield of 45%.

[0084] 1 H-NMR (400MHz, DMSO): δ8.62(m,1H,ArH),8.14-8.17(m,1H,ArH),8.03(m,1H,ArH),3.56(s,9H,CH3),3.47(t,2H,CH2),0.72-1.14(m,4H,CH2CH2);

[0085] LC / MS(ES,m / z):[M+H] + 324.6.

[0086] Example 2 Synthesis of Compound B1

[0087] 7.3 g (0.044 mol) of methyl 3,4-diaminobenzoate was dissolved in 100 mL of acetic acid, and 3.36 g (0.048 mol) of sodium nitrite was slowly added. The mixture was stirred at room temperature for 18 hours. After the reaction was complete, the reaction solution was poured into 300 mL of water, and the pH value was adjusted to neutral with sodium carbonate. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid with a yield of 78%.

[0088] 8.49 g (0.048 mol) of 1,2,3-benzotriazole-5-carboxylic acid methyl ester was dispersed in 100 mL of water, and 200 mL of sodium hydroxide solution was slowly added. The mixture was stirred at 40°C for 4 hours. After the reaction was complete, the mixture was cooled to room temperature, and the pH value was adjusted to neutral with hydrochloric acid. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid. The yield was 66%.

[0089] 9.1 g (0.056 mol) of 5-carboxylic acid benzotriazole was dissolved in 500 mL of dichloromethane, and 50 mL of oxalyl chloride was slowly added. The mixture was stirred at room temperature for 3 hours, and the solvent was evaporated under reduced pressure. The remaining reaction product was dissolved in 60 mL of dichloromethane to obtain a dichloromethane solution of 1H-benzothiazole-5-carbonyl chloride.

[0090] 10.76 g (0.06 mol) of 3-aminopropyltrimethoxysilane and 2.02 g (0.02 mol) of triethylamine were added to the above 60 mL of dichloromethane mixed solution, stirred at 30° C. for 6 hours, and the solvent was evaporated under reduced pressure. Compound B1 was obtained by column chromatography with a yield of 60%.

[0091] Example 3 Synthesis of Compound B1

[0092] 7.3 g (0.044 mol) of methyl 3,4-diaminobenzoate was dissolved in 100 mL of acetic acid, and 3.36 g (0.048 mol) of sodium nitrite was slowly added. The mixture was stirred at room temperature for 18 hours. After the reaction was complete, the reaction solution was poured into 300 mL of water, and the pH value was adjusted to neutral with sodium carbonate. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid with a yield of 75%.

[0093] 8.49 g (0.048 mol) of 1,2,3-benzotriazole-5-carboxylic acid methyl ester was dispersed in 100 mL of water, and 200 mL of sodium hydroxide solution was slowly added. The mixture was stirred at 40°C for 4 hours. After the reaction was complete, the mixture was cooled to room temperature, and the pH value was adjusted to neutral with hydrochloric acid. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid. The yield was 63%.

[0094] 9.1 g (0.056 mol) of 5-carboxylic acid benzotriazole was dissolved in 500 mL of dichloromethane, 100 mL of oxalyl chloride was slowly added, and the mixture was stirred at room temperature for 4 hours. The solvent was evaporated under reduced pressure, and the remaining reaction product was dissolved in 100 mL of dichloromethane to obtain a dichloromethane solution of 1H-benzothiazole-5-carbonyl chloride.

[0095] 10.76 g (0.06 mol) of 3-aminopropyltrimethoxysilane and 2.03 g (0.03 mol) of triethylamine were added to the above 100 mL of dichloromethane mixed solution, and the mixture was stirred at 60° C. for 3 hours. The solvent was evaporated under reduced pressure and compound B1 was obtained by column chromatography with a yield of 56%.

[0096] Example 4 Synthesis of Compound B2

[0097]

[0098] 7.3 g (0.044 mol) of methyl 3,4-diaminobenzoate was dissolved in 100 mL of acetic acid, and 3.36 g (0.048 mol) of sodium nitrite was slowly added. The mixture was stirred at room temperature for 18 hours. After the reaction was complete, the reaction solution was poured into 300 mL of water, and the pH value was adjusted to neutral with sodium carbonate. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid with a yield of 76%.

[0099] 8.49 g (0.048 mol) of 1,2,3-benzotriazole-5-carboxylic acid methyl ester was dispersed in 100 mL of water, and 200 mL of sodium hydroxide solution was slowly added. The mixture was stirred at 40°C for 4 hours. After the reaction was complete, the mixture was cooled to room temperature, and the pH value was adjusted to neutral with hydrochloric acid. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid. The yield was 65%.

[0100] 9.1 g (0.056 mol) of 5-carboxylic acid benzotriazole was dissolved in 500 mL of dichloromethane, and 50 mL of oxalyl chloride was slowly added. The mixture was stirred at room temperature for 3 hours, and the solvent was evaporated under reduced pressure. The remaining reaction product was dissolved in 60 mL of dichloromethane to obtain a dichloromethane solution of 1H-benzothiazole-5-carbonyl chloride.

[0101] 11.77 g (0.05 mol) of 4-aminobutyltriethoxysilane and 2.02 g (0.02 mol) of triethylamine were added to the above 60 mL of dichloromethane mixed solution, stirred at 30° C. for 6 hours, and the solvent was evaporated under reduced pressure. Compound B2 was obtained by column chromatography with a yield of 54%.

[0102] 1 H-NMR (400MHz, DMSO): δ8.67(m,1H,ArH),8.10-8.15(m,1H,ArH),8.03(m,1H,ArH).3.85(q,6H ,OCH2),3.35(t,2H,CH2NH),1.41-1.53(m,4H,CH2CH2),1.25(t,9H,CH3),0.56(t,2H,CH2Si);

[0103] LC / MS(ES,m / z):[M+H] + 380.5.

[0104] Example 5 Synthesis of Compound B3

[0105]

[0106] 7.3 g (0.044 mol) of methyl 3,4-diaminobenzoate was dissolved in 100 mL of acetic acid, and 3.36 g (0.048 mol) of sodium nitrite was slowly added. The mixture was stirred at room temperature for 18 hours. After the reaction was complete, the reaction solution was poured into 300 mL of water, and the pH value was adjusted to neutral with sodium carbonate. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid with a yield of 73%.

[0107] 8.49 g (0.048 mol) of 1,2,3-benzotriazole-5-carboxylic acid methyl ester was dispersed in 100 mL of water, and 200 mL of sodium hydroxide solution was slowly added. The mixture was stirred at 40°C for 4 hours. After the reaction was complete, the mixture was cooled to room temperature, and the pH value was adjusted to neutral with hydrochloric acid. The mixture was extracted with 500 mL of ethyl acetate, dried with anhydrous sodium sulfate, and purified by column chromatography to obtain an off-white solid. The yield was 64%.

[0108] 9.1 g (0.056 mol) of 5-carboxylic acid benzotriazole was dissolved in 500 mL of dichloromethane, and 50 mL of oxalyl chloride was slowly added. The mixture was stirred at room temperature for 3 hours, and the solvent was evaporated under reduced pressure. The remaining reaction product was dissolved in 60 mL of dichloromethane to obtain a dichloromethane solution of 1H-benzothiazole-5-carbonyl chloride.

[0109] 11.07 g (0.05 mol) of 3-aminopropyltriethoxysilane and 20.2 g (0.2 mol) of triethylamine were added to the above 60 mL of dichloromethane mixed solution, stirred at 30° C. for 6 hours, and the solvent was evaporated under reduced pressure. Compound B3 was obtained by column chromatography with a yield of 55%.

[0110] 1H-NMR (400MHz, DMSO): δ8.72(m,1H,ArH),8.23(m,1H,ArH),8.11(m,1H,ArH),3.94(q, 6H,CH2O),3.50(t,2H,CH2NH),1.55(m,2H,CH2),1.22(t,9H,CH3),0.63(t,2H,CH2Si);

[0111] LC / MS(ES,m / z):[M+H] + 367.5.

[0112] Example 6 Preparation of Carbon Coated Copper Foil

[0113] Carbon coating slurry formula includes:

[0114] Conductive agent: 2 parts of graphite KS-6, 8 parts of carbon black SP;

[0115] Dispersant: 2 parts BYK22092;

[0116] Dispersing aid: 1 part propylene glycol methyl ether;

[0117] Binder: 0.5 parts of compound B1 binder;

[0118] The rest is solvent water.

[0119] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 20 minutes at a speed of 300 r / min, then the conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and finally the product B1 binder is added, sand milled for 1 hour at a speed of 600 r / min, and discharged.

[0120] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 60mm / s;

[0121] Drying: Dry at 80°C for 5 min to obtain the sample.

[0122] Example 7 Preparation of Carbon Coated Copper Foil

[0123] Carbon coating slurry formula includes:

[0124] Conductive agent: 5 parts of graphite KS-6, 5 parts of carbon black SP;

[0125] Dispersant: 0.8 parts BYK22092;

[0126] Dispersing aid: 0.5 parts of tert-butyl alcohol;

[0127] Binder: 1 part of compound B1 binder;

[0128] The rest is solvent water.

[0129] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 500 r / min, then the conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and finally the product B1 binder is added, sand milled for 1 hour at a speed of 600 r / min, and discharged.

[0130] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 60mm / s;

[0131] Drying: Dry at 120°C for 3 min to obtain a sample.

[0132] Example 8 Preparation of Carbon Coated Copper Foil

[0133] Carbon coating slurry formula includes:

[0134] Conductive agent: 9 parts of graphite KS-6, 1 part of carbon black SP;

[0135] Dispersant: 0.5 parts BYK019;

[0136] Dispersing aid: 0.1 part of propylene glycol methyl ether;

[0137] Binder: 2 parts of compound B1 binder;

[0138] The rest is solvent water.

[0139] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 40 minutes at a speed of 200 r / min, then the conductive agent is added, sand milled for 6 hours at a speed of 600 r / min, and finally the product B1 binder is added, sand milled for 2 hours at a speed of 600 r / min, and discharged.

[0140] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 80mm / s;

[0141] Drying: Dry at 120°C for 2 min to obtain a sample.

[0142] Example 9 Preparation of Carbon Coated Copper Foil

[0143] Carbon coating slurry formula includes:

[0144] Conductive agent: 8 parts of graphite KS-6, 2 parts of carbon black SP;

[0145] Dispersant: 1 part BYK440;

[0146] Dispersing aid: 0.3 parts of tert-butyl alcohol;

[0147] Binder: 1 part of compound B2 binder;

[0148] The rest is solvent water.

[0149] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 500 r / min, then the conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and finally the product B2 binder is added, sand milled for 1 hour at a speed of 600 r / min, and discharged.

[0150] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 80mm / s;

[0151] Drying: Dry at 120°C for 3 min to obtain a sample.

[0152] Example 10 Preparation of Carbon Coated Copper Foil

[0153] Carbon coating slurry formula includes:

[0154] Conductive agent: 4 parts of graphite KS-6, 6 parts of carbon black SP;

[0155] Dispersant: 1 part BYK206;

[0156] Dispersing aid: 0.5 parts of propylene glycol butyl ether;

[0157] Binder: 1.5 parts of compound B2 binder;

[0158] The rest is solvent water.

[0159] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 40 minutes at a speed of 600 r / min, followed by adding conductive agent, sand milling for 3 hours at a speed of 800 r / min, and finally adding product B2 binder, sand milling for 1 hour at a speed of 500 r / min, and discharging.

[0160] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 80mm / s;

[0161] Drying: Dry at 120°C for 3 min to obtain a sample.

[0162] Example 11 Preparation of Carbon-Coated Copper Foil

[0163] Carbon coating slurry formula includes:

[0164] Conductive agent: 1 part graphite KS-6, 9 parts carbon black SP;

[0165] Dispersant: 1 part BYK440;

[0166] Dispersing aid: 0.5 parts of isopropanol;

[0167] Binder: 1 part of compound B3 binder;

[0168] The rest is solvent water.

[0169] Preparation process: Add dispersant and dispersing aid into solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 600 r / min, then add conductive agent, sand grind for 4 hours at a speed of 800 r / min, finally add product B2 binder, sand grind for 1 hour at a speed of 500 r / min, and discharge.

[0170] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 80mm / s;

[0171] Drying: Dry at 120°C for 3 min to obtain a sample.

[0172] Example 12 Preparation of Carbon-Coated Copper Foil

[0173] Carbon coating slurry formula includes:

[0174] Conductive agent: 7 parts of graphite KS-6, 3 parts of carbon black SP;

[0175] Dispersant: 1 part BYK22092;

[0176] Dispersing aid: 0.5 parts of tert-butyl alcohol;

[0177] Binder: 2 parts of compound B3 binder;

[0178] The rest is solvent water.

[0179] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 40 minutes at a speed of 600 r / min, then the conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and finally the product B2 binder is added, sand milled for 1 hour at a speed of 500 r / min, and discharged.

[0180] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 80mm / s;

[0181] Drying: Dry at 120°C for 3 min to obtain a sample.

[0182] Comparative Example 1

[0183] Carbon coating slurry formula includes:

[0184] Conductive agent: 5 parts of graphite KS-6, 5 parts of carbon black SP;

[0185] Dispersant: 0.8 parts BYK22092;

[0186] Dispersing aid: 0.5 parts of tert-butyl alcohol;

[0187] Binder: 1 part 3-aminopropyltrimethoxysilane, 1 part benzotriazole;

[0188] The rest is solvent water.

[0189] Preparation process: Add dispersant and dispersing aid into solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 500r / min, then add conductive agent, sand grind for 4 hours at a speed of 1000r / min, finally add binder, sand grind for 1 hour at a speed of 600r / min, and discharge.

[0190] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 60mm / s;

[0191] Drying: Dry at 120°C for 3 min to obtain a sample.

[0192] Comparative Example 2

[0193] Carbon coating slurry formula includes:

[0194] Conductive agent: 5 parts of graphite KS-6, 5 parts of carbon black SP;

[0195] Dispersant: 0.8 parts BYK22092;

[0196] Dispersing aid: 0.5 parts of tert-butyl alcohol;

[0197] Binder: 0.3 parts of compound B1 binder;

[0198] The rest is solvent water.

[0199] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 500 r / min, then the conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and finally the product B1 binder is added, sand milled for 1 hour at a speed of 600 r / min, and discharged.

[0200] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 60mm / s;

[0201] Drying: Dry at 120°C for 3 min to obtain a sample.

[0202] Comparative Example 3

[0203] Carbon coating slurry formula includes:

[0204] Conductive agent: 5 parts of graphite KS-6, 5 parts of carbon black SP;

[0205] Dispersant: 0.8 parts BYK22092;

[0206] Dispersing aid: 0.5 parts of tert-butyl alcohol;

[0207] Binder: 3 parts of compound B1 binder;

[0208] The rest is solvent water.

[0209] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 500 r / min, then the conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and finally the product B1 binder is added, sand milled for 1 hour at a speed of 600 r / min, and discharged.

[0210] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 60mm / s;

[0211] Drying: Dry at 120°C for 3 min to obtain a sample.

[0212] Comparative Example 4

[0213] Copper foil pretreatment: Add 1 part of 3-aminopropyltrimethoxysilane and 1 part of 1H-benzothiazole-5-carbonyl chloride into deionized water, stir evenly, and prepare a concentration of 1×10 -4mol / L mixed solution, and then coated the mixed solution on the copper foil with a 5μm wire rod at a coating speed of 60mm / s, followed by drying at 120℃ for 3min to obtain the pretreated copper foil.

[0214] Carbon coating slurry formula includes:

[0215] Conductive agent: 5 parts of graphite KS-6, 5 parts of carbon black SP;

[0216] Dispersant: 0.8 parts BYK22092;

[0217] Dispersing aid: 0.5 parts of tert-butyl alcohol;

[0218] The rest is solvent water.

[0219] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 500 r / min, and then a conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and then discharged.

[0220] Coating: Place an appropriate amount of carbon coating slurry on the pretreated copper foil and apply it with a 5μm wire rod at a coating speed of 60mm / s;

[0221] Drying: Dry at 120°C for 3 min to obtain a sample.

[0222] Comparative Example 5

[0223] Carbon coating slurry formula includes:

[0224] Conductive agent: 5 parts of graphite KS-6, 5 parts of carbon black SP;

[0225] Dispersant: 0.8 parts BYK22092;

[0226] Dispersing aid: 0.5 parts of tert-butyl alcohol;

[0227] Binder: 1 part of Compound C Binder;

[0228] The rest is solvent water.

[0229] The structural formula of compound C is as follows:

[0230]

[0231] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 500 r / min, then the conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and finally the product B1 binder is added, sand milled for 1 hour at a speed of 600 r / min, and discharged.

[0232] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 60mm / s;

[0233] Drying: Dry at 120°C for 3 min to obtain a sample.

[0234] Comparative Example 6

[0235] Carbon coating slurry formula includes:

[0236] Conductive agent: 5 parts of graphite KS-6, 5 parts of carbon black SP;

[0237] Dispersant: 0.8 parts BYK22092;

[0238] Dispersing aid: 0.5 parts of tert-butyl alcohol;

[0239] Adhesive: 1 part commercially available acrylic adhesive;

[0240] The rest is solvent water.

[0241] Preparation process: Dispersant and dispersing aid are added to solvent water at the same time for high-speed dispersion for 30 minutes at a speed of 500 r / min, then the conductive agent is added, sand milled for 4 hours at a speed of 1000 r / min, and finally the product B1 binder is added, sand milled for 1 hour at a speed of 600 r / min, and discharged.

[0242] Coating: Place an appropriate amount of carbon coating slurry on the copper foil and apply it with a 5μm wire rod at a coating speed of 60mm / s;

[0243] Drying: Dry at 120°C for 3 min to obtain a sample.

[0244] The peel strength, square resistance, water wiping resistance and NMP wiping resistance of carbon-coated copper foil were tested. The results are as follows:

[0245] Example <![CDATA[Peeling strength / N·m -1 > Square resistance Water resistant NMP wiping resistance Example 6 80 2.0mΩ / □ 200 times without showing your bottom 200 times without showing your bottom Example 7 89 1.9mΩ / □ 200 times without showing your bottom 200 times without showing your bottom Example 8 90 2.2mΩ / □ 200 times without showing your bottom 200 times without showing your bottom Example 9 86 2.1mΩ / □ 200 times without showing your bottom 200 times without showing your bottom Example 10 88 2.0mΩ / □ 200 times without showing your bottom 200 times without showing your bottom Embodiment 11 85 1.9mΩ / □ 200 times without showing your bottom 200 times without showing your bottom Example 12 92 2.3mΩ / □ 200 times without showing your bottom 200 times without showing your bottom Comparative Example 1 39 5.0mΩ / □ Exposed Exposed Comparative Example 2 53 1.8mΩ / □ Partially exposed Partially exposed Comparative Example 3 95 2.3mΩ / □ 200 times without showing your bottom 200 times without showing your bottom Comparative Example 4 3 1539Ω / □ Exposed Exposed Comparative Example 5 38 2.1mΩ / □ Exposed Exposed Comparative Example 6 43 2.0mΩ / □ Exposed Exposed

[0246] From the above results, it can be seen that the homemade adhesive has excellent adhesion and extremely low resistance (Examples 6-12), and its peel strength exceeds 80N·m -1, the square resistance is within the range of 2.3mΩ / □, and the water wiping resistance and NMP wiping resistance are excellent. The amount of homemade adhesive needs to be appropriate (Comparative Examples 2-3). Too little affects the performance, and too much increases the cost. In addition, the homemade adhesive is not simply superimposed and compounded. The homemade adhesive has a special structure and has special requirements for the structure (Comparative Example 1, Comparative Example 4, Comparative Example 5). In Comparative Example 1, a binder is added in a simple compounding manner, and the binder does not play a synergistic effect, does not effectively improve the adhesion between the copper foil and the conductive agent, but increases unnecessary internal resistance; Comparative Example 4 forms a dense layer on the surface of the copper foil, the dense layer has extremely poor conductivity, and the dense layer cannot be effectively bonded to the conductive agent, resulting in extremely large square resistance and extremely low peel strength; In Comparative Example 5, if other segments are grafted on the N atom of benzotriazole, such as the above-mentioned compound C, the grafted segments first occupy an N atom used to form a covalent bond and a coordination bond with the copper atom, making it impossible to form a chain polymer with the copper atom, and secondly, the generated steric effect affects the formation of the covalent bonds and coordination bonds of the other two N atoms, thereby greatly affecting the adhesion between benzotriazole and copper, so there are special restrictions on the structure of the homemade binder. In addition, compared with the commercially available binder (Comparative Example 6), the peel strength of the homemade binder is significantly higher and the binder is strong when the amount of binder is very small.

[0247] In summary, the homemade adhesive can ensure the strong adhesion and low resistance of the carbon-coated foil when used in a small amount, and has excellent water wiping resistance and NMP wiping resistance, which can significantly reduce the cost and has practical significance for the development of carbon-coated foil.

Claims

1. A compound, characterized in that is a compound as shown in formula (I), (I); in: R1 is C 1-4 Alkyl, R2 is C 1-6 Alkylene.

2. The compound according to claim 1, characterized in that The R1 is methyl, ethyl, n-propyl, isopropyl, n-butyl or isobutyl; the R2 is methylene, 1,2-ethylene, 1,3-propylene, 2-methyl-1,3-propylene, 1,4-butylene or 2,2-dimethyl-1,4-butylene.

3. A compound, characterized in that The compound has one of the following structures: 、 、 、 、 、 、 、 、 、 。 4. A binder for carbon-coated copper foil, characterized in that: Contains one or more of the compounds described in any one of claims 1 to 3.

5. A method for preparing a carbon-coated copper foil, characterized in that: The following steps are involved: S1. Prepare carbon coating slurry: add dispersant and dispersing aid into solvent for dispersion, add conductive agent, and finally add binder as claimed in claim 4 to obtain carbon coating slurry; wherein, the dispersant is one or more of BYK22092 and BYK206; the dispersing aid is one or more of ethanol, n-butanol, tert-butanol, n-propanol, isopropanol, propylene glycol methyl ether, propylene glycol butyl ether; S2, coating: taking the above carbon coating slurry and coating it on the copper foil; S3, drying: drying the coated copper foil to obtain the carbon-coated copper foil.

6. The preparation method according to claim 5, characterized in that: In the step S1, the binder is 0.5 to 2 parts by weight based on 100 parts by total weight of the carbon coating slurry.

7. The preparation method according to claim 5, characterized in that: In the step S1, based on the total weight of the carbon coating slurry being 100 parts, the dispersant is 0.1 to 2 parts, the dispersing aid is 0.1 to 1 part, the conductive agent is 2 to 18 parts, and the rest is solvent; wherein the solvent is water.

8. The preparation method according to claim 5, characterized in that: The conductive agent is one or more of graphite, carbon black, carbon nanotubes and graphene.

9. A carbon-coated copper foil, characterized in that: The invention is prepared by the preparation method according to any one of claims 5 to 8.

10. A lithium battery, characterized in that: A carbon-coated copper foil prepared by the preparation method according to any one of claims 5 to 8.