Polypropylene composition, preparation method and application thereof, polyolefin microporous breathable film

By using maleic anhydride copolymer microspheres as porogens in polypropylene microporous membranes, the problems of uneven particle size and strong hydrophobicity of the porogens in polypropylene microporous membranes are solved, and the air permeability and performance of the breathable membranes are improved. Hydrophilic, suitable for medical and sanitary products and waterproof and breathable materials.

CN116063725BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202111272457.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-15
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Existing polypropylene microporous membranes have problems such as uneven particle size, poor dispersion, poor compatibility, and strong hydrophobicity during the preparation process, which leads to problems with breathability and biological contamination, limiting its use in medical and food products. Applications in packaging and other fields.

Method used

Maleic anhydride copolymer microspheres are used as organic porogens. Through melt blending, extrusion, pelletizing and drying in a twin-screw extruder, the porogens are evenly dispersed in polypropylene to avoid coupling. The use of agents and dispersants can improve the breathability uniformity and hydrophilicity of the breathable membrane.

Benefits of technology

It achieves the uniform dispersion of porogen in polypropylene, improves the uniformity and air permeability of the breathable film, solves the problems of small adjustable range of air permeability and biological contamination in the existing technology, and is suitable for disposable medical and sanitary products and waterproof and breathable materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116063725B_ABST
    Figure CN116063725B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of polyolefin compositions, and discloses a polyolefin composition and its preparation method and application. The composition includes polypropylene, a porogen and an antioxidant composite auxiliary agent; based on 100 parts by weight of polypropylene, the amount of the porogen is 50-120 parts by weight, and the amount of the antioxidant composite auxiliary agent is 0.1-2 parts by weight; the porogen is maleic anhydride copolymer microspheres, and the average particle size of the copolymer microspheres is 500-1600nm. The composition uses maleic anhydride copolymer microspheres as organic porogens, and the particle size distribution of the copolymer microspheres is uniform, and can be evenly dispersed in polypropylene without using coupling agents and dispersants, and no agglomeration phenomenon occurs, thereby being able to avoid the shortcomings of uneven pore size distribution, poor dispersibility, poor compatibility, etc. caused by inorganic porogens, and the composition is also hydrophilic. It is used in a breathable film, and the air permeability uniformity and air permeability of the breathable film can be significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polypropylene composition, in particular to a polypropylene composition and a preparation method and application thereof, and a polyolefin microporous breathable film. Background Art

[0002] Polypropylene microporous membrane is a composite material made of polypropylene as raw material, filled with a certain proportion of solid particles (such as calcium carbonate, barium sulfate, titanium dioxide, talcum powder and other mineral fillers), and made into a film by blowing, calendering or casting, and then a large number of small and interconnected microporous membranes with a diameter between 0.01-10μm are obtained by uniaxial or biaxial stretching under appropriate conditions. Therefore, water droplets with a diameter of about 100μm cannot penetrate the pores on the surface of the microporous membrane. If there is an appropriate concentration gradient on the inner and outer surfaces of the membrane, water vapor, air and other gases with a diameter of 0.0004μm can freely pass through the tortuous channels through diffusion and convection. Polypropylene microporous membrane has efficient separation ability and excellent mechanical properties, so it has been widely used in the fields of medical and industrial breathable membranes, microfiltration membranes, ultrafiltration membranes, separation membranes, battery diaphragms, capacitor diaphragms, etc.

[0003] CN100362027C discloses a special material for polyolefin antibacterial breathable film and a preparation method thereof. After 10-30 parts of nano calcium carbonate and 10-65 parts of heavy calcium carbonate are mixed, long fatty chain monomers, initiators, polyether sulfonates and macromolecular coupling agents are added for treatment, and then mixed with 5-80 parts of polyolefin resin in a twin-screw extruder to prepare a pre-dispersed masterbatch of mixed calcium carbonate, and then mixed with a pore leveling agent, an antioxidant, an antibacterial masterbatch and a polyolefin resin, and extruded and granulated to obtain an antibacterial special material for polyolefin breathable film. The material contains a certain amount of amino silicone oil as a pore leveling agent, which is easy to form die head smoke in the film making process, and then forms die head oil droplets and fouling, thereby causing longitudinal stripes and oil droplet pollution on the film surface. In addition, although nano calcium carbonate and heavy calcium carbonate are first made into masterbatch and then granulated with other components through a twin-screw extruder, although it is conducive to the dispersion of fillers, the process is complicated and the processing cost is high.

[0004] In order to improve the bonding force between inorganic particles and organic polymers, coupling agents are often added. However, coupling agents are easily decomposed by heat during high-temperature processing to produce small molecules, which evaporate into the air and produce unpleasant odors. This is not in line with the environmental protection concept of clean production and also limits the application of products in medical and sanitary materials and food packaging.

[0005] At present, inorganic porogens used in the production of breathable membranes on the market still have the following problems: (1) easy to agglomerate; (2) due to the large particle size and uneven particle size distribution, the pore size uniformity of the breathable membrane is poor, and even a large number of pinhole defects appear; (3) the surface modification effect of the filler particles is poor, and the compatibility with the matrix is ​​poor, thus affecting the strength of the film; (4) the filler particles have poor dispersion and will migrate to the surface of the breathable membrane, causing color difference or color spots on the breathable membrane.

[0006] On the other hand, since the surface of polypropylene does not contain polar groups, its surface energy is very small, and the critical surface tension is only 31-34×10 -5 N / cm, so it is hydrophobic. When polypropylene is prepared into a microporous membrane, it will show stronger hydrophobicity, so that water vapor needs a higher pressure to pass through; it is also easy to adsorb proteins and bacteria during use, resulting in biological contamination of the membrane, greatly reducing the water flux and separation selectivity of the membrane. Therefore, hydrophilic modification of the membrane is an important method to improve the water flux and pollution resistance of the membrane, which is also one of the research hotspots of membrane materials today. Summary of the invention

[0007] In order to overcome the problems existing in the prior art, the present invention provides a polypropylene composition and a preparation method and application thereof, and a polyolefin microporous breathable film. The composition comprises organic porogen maleic anhydride copolymer microspheres, the particle size distribution of the copolymer microspheres is uniform, and can be uniformly dispersed in polypropylene without using a coupling agent or a dispersant, and there is no agglomeration phenomenon, thereby avoiding the shortcomings of uneven pore size distribution, poor dispersibility, poor compatibility, etc. caused by inorganic porogens, and the composition is also hydrophilic. When used in a breathable film, the air permeability uniformity and air permeability of the breathable film can be significantly improved.

[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a polypropylene composition, characterized in that the composition comprises polypropylene, a porogen and an antioxidant composite auxiliary agent;

[0009] Based on 100 parts by weight of polypropylene, the amount of the porogen is 50-120 parts by weight, and the amount of the antioxidant composite auxiliary is 0.1-2 parts by weight;

[0010] The porogen is maleic anhydride copolymer microspheres, and the average particle size of the maleic anhydride copolymer microspheres is 500-1600nm.

[0011] The second aspect of the present invention provides use of the polypropylene composition in a polyolefin microporous breathable film.

[0012] The third aspect of the present invention provides a method for preparing the above-mentioned polypropylene composition, characterized in that the method comprises:

[0013] (1) mixing polypropylene, a porogen and an antioxidant composite auxiliary agent to obtain a mixture;

[0014] (2) The mixture is melt-blended, extruded, pelletized and dried in a twin-screw extruder to obtain the polypropylene composition.

[0015] A fourth aspect of the present invention provides a polyolefin microporous breathable membrane, characterized in that the microporous breathable membrane is made from the above-mentioned polypropylene composition.

[0016] Through the above technical scheme, the polypropylene composition, preparation method and application thereof, and polyolefin microporous breathable film provided by the present invention achieve the following beneficial effects:

[0017] Maleic anhydride copolymer microspheres are added to the polypropylene composition provided by the present invention as an organic porogen, and the porogen is evenly dispersed in the polypropylene without using a coupling agent and a dispersant, and the pore size of the micropores is uniform; the polypropylene composition of the present invention is also hydrophilic, and can solve the problem of small adjustable range of physical properties and air permeability of the breathable membrane in the prior art, and has wide adaptability, simple operation and stable product performance.

[0018] The polypropylene composition prepared by the present invention can be widely used in the fields of disposable medical and sanitary products, waterproof and breathable materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a SEM photograph of a cross section of a polypropylene composition sample obtained in Example 1;

[0020] Figure 2 is a SEM photograph of a cross section of a polypropylene composition sample obtained in Example 2;

[0021] Figure 3 is a SEM photograph of a cross section of a polypropylene composition sample obtained in Example 3;

[0022] Figure 4 This is a SEM photo of the cross section of the polypropylene composition sample obtained in Example 5.

[0023] Figure 5 is a SEM photograph of a cross section of a polypropylene composition sample obtained in Comparative Example 1;

[0024] Figure 6 is a SEM photograph of a cross section of a polypropylene composition sample obtained in Comparative Example 2;

[0025] Figure 7 This is a SEM photograph of the cross section of the polypropylene composition sample prepared in Comparative Example 3. DETAILED DESCRIPTION

[0026] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0027] The first aspect of the present invention provides a polypropylene composition, characterized in that the composition comprises polypropylene, a porogen and an antioxidant composite auxiliary agent;

[0028] Based on 100 parts by weight of polypropylene, the amount of the porogen is 50-120 parts by weight, and the amount of the antioxidant composite auxiliary is 0.1-2 parts by weight;

[0029] The porogen is maleic anhydride copolymer microspheres, and the average particle size of the maleic anhydride copolymer microspheres is 500-1600nm.

[0030] Maleic anhydride copolymer microspheres are added to the composition provided by the invention as a porogen, and the particle size distribution of the copolymer microspheres is uniform, and the porogen can be evenly dispersed in polypropylene without using a coupling agent or a dispersant, and the pore size of the micropores is uniform; the problem that the physical properties and the air permeability of the breathable membrane in the prior art have a small adjustable range can be solved, and the invention has wide adaptability, simple operation, and stable product performance.

[0031] Furthermore, based on 100 parts by weight of polypropylene, the amount of the porogen is 60-110 parts by weight, and the amount of the antioxidant composite auxiliary is 0.2-1.8 parts by weight.

[0032] Furthermore, the average particle size of the maleic anhydride copolymer microspheres is 600-1300 nm, preferably 600-1200 nm.

[0033] According to the present invention, the melting enthalpy of the polypropylene is ΔH mPP , the melting enthalpy of the polypropylene composition is ΔH m组合物 ;

[0034] Among them, △H mPP With △H m组合物 The difference is 15-38J / g.

[0035] In the present invention, when the difference between the melting enthalpy of the polypropylene and the melting enthalpy of the polypropylene composition satisfies the above range, it can be shown that the maleic anhydride copolymer microspheres are evenly distributed in the polypropylene composition, and there is no significant decrease in the melting enthalpy of the composition due to agglomeration of the maleic anhydride copolymer microspheres, thereby making the breathable film prepared from the composition have both excellent physical properties and breathability.

[0036] In the present invention, the melting enthalpy of the polypropylene and the polypropylene composition is measured by differential scanning calorimetry.

[0037] Furthermore, △H mPP With △H m组合物 The difference is 18-32 J / g.

[0038] According to the present invention, the copolymer in the maleic anhydride copolymer microspheres comprises a structural unit A derived from maleic anhydride and a structural unit B derived from a comonomer, and based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 48-55%, and the molar content of the structural unit B is 45-52%.

[0039] According to the present invention, the comonomer is selected from at least one of styrene, α-methylstyrene, vinyl acetate, C4 olefins and C5 olefins.

[0040] In the present invention, the mixed C4 refers to a general term for hydrocarbon compounds with four carbon atoms (mainly including butene). Generally, in addition to butenes of various structures (such as trans-2-butene, cis-2-butene, normal butene, isobutene), the C4 also includes a certain amount of alkanes (such as normal butane) and other impurities that may exist. In the present invention, the content of olefins in the mixed C4 is within the range of 60-75% by weight.

[0041] In the present invention, the mixed C5 refers to a general term for hydrocarbon compounds with five carbon atoms (mainly including pentenes). Generally, in addition to various pentenes of different structures (such as dienes (isoprene, cyclopentadiene, 1,4-pentadiene, piperylene) and monoolefins (1-pentene, 2-pentene, cyclopentene, 2-methyl-1-butene, 2-methyl-2-butene)), the C5 also includes a certain amount of alkanes (such as n-pentane, isopentane, cyclopentane, 2-methylbutane), alkynes (such as butyne-2, 3-pentene-1yne) and other impurities that may exist. In the present invention, the content of olefins in the mixed C5 is 55-65% by weight.

[0042] According to the present invention, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 48-53%, preferably 49-51%, and the molar content of the structural unit B is 47-52%, preferably 49-51%.

[0043] In one specific embodiment of the present invention, the porogen is maleic anhydride styrene copolymer microspheres, which are prepared according to the following steps:

[0044] (1) dissolving maleic anhydride, comonomer and initiator in a reaction medium in an inert atmosphere to form a homogeneous solution;

[0045] (2) the homogeneous solution is subjected to a polymerization reaction to obtain a copolymer emulsion suspension, and then the porogen is obtained after solid-liquid separation;

[0046] Wherein, based on the total weight of maleic anhydride and the comonomer, the amount of maleic anhydride is 50-90wt%, and the amount of the comonomer is 10-50wt%;

[0047] The reaction medium is a mixture of the compound represented by formula (1) and an alkane;

[0048]

[0049] Wherein, R1 and R2 are each independently an alkyl group having 1 to 6 carbon atoms.

[0050] In a specific embodiment of the present invention, the comonomer is selected from at least one of styrene, α-methylstyrene and vinyl acetate.

[0051] In the present invention, maleic anhydride monomer and comonomer are copolymerized in a specific ratio, so that the prepared maleic anhydride copolymer is in the form of microspheres with excellent uniformity, and the copolymer has the characteristics of clean surface, good dispersibility in the medium and no aggregation.

[0052] Furthermore, in order to obtain maleic anhydride copolymer microspheres with uniform particles and excellent morphology, the inventors studied the dosage of maleic anhydride and comonomers during the polymerization process. The study showed that when the dosage of maleic anhydride is 50-60wt% and the dosage of the comonomer is 40-50wt% based on the total weight of the polymerized monomers, the obtained maleic anhydride copolymer microspheres have uniform particles, excellent particle morphology, and a clean particle surface, and the comprehensive performance of the copolymer microspheres is even better.

[0053] According to the present invention, based on the total weight of the homogeneous solution, the total mass concentration of the maleic anhydride and the comonomer is 5-25 wt %, preferably 5-20 wt %.

[0054] According to the present invention, the initiator is an organic peroxide and / or an azo compound.

[0055] According to the present invention, the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate.

[0056] According to the present invention, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.

[0057] According to the present invention, based on the total weight of the homogeneous solution, the mass concentration of the initiator is 0.01-5wt%, preferably 1-4wt%.

[0058] According to the present invention, in formula (1), R1 and R2 are each independently an alkyl group having 1 to 4 carbon atoms, more preferably a methyl group or an ethyl group.

[0059] According to the present invention, the alkane is an alkane having 6 to 12 carbon atoms.

[0060] In the present invention, a mixture of the compound represented by formula (1) and an alkane is selected as the reaction medium, which can cooperate with the specific amount of maleic anhydride and the comonomer described in the present invention to achieve a self-stabilizing precipitation polymerization reaction of maleic anhydride and the comonomer. The polymerization reaction system does not need to add any stabilizer or co-stabilizer, has a self-stabilizing dispersion effect, and the surface of the obtained polymer microspheres is clean and pollution-free.

[0061] Furthermore, the alkane is at least one selected from hexane, heptane and octane, more preferably hexane.

[0062] According to the present invention, the amount of the alkane used is 50-90 vol%, preferably 60-80 vol%, based on the total volume of the reaction medium.

[0063] In the present invention, the polymerization reaction is carried out in an inert atmosphere, and the inert atmosphere can be provided by conventional inert gases in the prior art, such as nitrogen.

[0064] According to the present invention, the conditions of the polymerization reaction include: the polymerization temperature is 61-100° C., preferably 70-90° C.; the polymerization time is 1-24 h, preferably 2-12 h.

[0065] In the present invention, a water bath and / or an oil bath is used to provide the heat required for the polymerization of the present invention.

[0066] In the present invention, the solid-liquid separation may be a conventional solid-liquid separation method in the art, such as centrifugal separation.

[0067] In the present invention, when centrifugal separation is adopted, the centrifugal speed is 1500-5000 rad / min, and the centrifugal time is 5-60 min.

[0068] In one embodiment of the present invention, the porogen is maleic anhydride copolymer microspheres, which are prepared according to the following steps:

[0069] In the presence of an inert atmosphere, an initiator and an organic solvent, maleic anhydride and a comonomer are copolymerized to obtain the maleic anhydride copolymer microspheres;

[0070] The comonomer is selected from mixed C4 and / or mixed C5.

[0071] In the present invention, the copolymerization reaction may be a one-step reaction using a precipitation polymerization method.

[0072] According to the present invention, the weight ratio of the maleic anhydride to the comonomer is 1:(0.2-3); preferably 1:(0.8-3).

[0073] According to the present invention, based on the total amount of maleic anhydride, the amount of the initiator is 0.05-20 mol%.

[0074] According to the present invention, the organic solvent is selected from at least one of isoamyl acetate, butyl acetate, isopropyl acetate and ethyl acetate. Preferably, based on the total weight of the organic solvent, the concentration of maleic anhydride is 5-25wt%; preferably 10-20wt%.

[0075] According to the present invention, the copolymerization reaction conditions are: copolymerization reaction temperature is 50-100°C, preferably 70-90°C; copolymerization reaction pressure is 0.2-2MPa, preferably 0.5-1MPa; copolymerization reaction time is 5-10h, preferably 6-9h.

[0076] According to the present invention, the initiator is an organic peroxide and / or an azo compound.

[0077] According to the present invention, the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate.

[0078] According to the present invention, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.

[0079] In the present invention, a water bath and / or an oil bath is used to provide the heat required for the polymerization of the present invention.

[0080] In the present invention, the solid-liquid separation may be a conventional solid-liquid separation method in the art, such as centrifugal separation or flash separation.

[0081] In the present invention, when centrifugal separation is adopted, the centrifugal speed is 1500-5000 rad / min, and the centrifugal time is 5-60 min.

[0082] In the present invention, when flash separation is adopted, it can be carried out in a flash separator, the flash temperature is 10-40° C., and the flash pressure is 0 MPa.

[0083] According to the present invention, the polypropylene is a propylene homopolymer or a mixture of a propylene homopolymer and a heterophasic propylene copolymer.

[0084] According to the present invention, based on 100 parts by weight of polypropylene, the amount of the propylene homopolymer is 60-95 parts by weight, preferably 70-95 parts by weight; the amount of the heterophasic propylene copolymer is 5-40 parts by weight, preferably 5-30 parts by weight.

[0085] According to the present invention, the isotacticity of the propylene homopolymer is 95-99.5%, preferably 96-99.5%.

[0086] According to the present invention, the xylene soluble content of the propylene homopolymer is 0.3-5wt%, preferably 0.5-4wt%.

[0087] According to the present invention, the melt flow rate of the propylene homopolymer at 230°C and a load of 2.16 kg is 0.5 g / 10min-10 g / 10min, preferably 2 g / 10min-6 g / 10min;

[0088] According to the present invention, the molecular weight distribution of the propylene homopolymer is 1-10, preferably 2-6.

[0089] According to the present invention the heterophasic propylene copolymer comprises 60 to 99 wt% of structural units I provided by propylene and 1 to 40 wt% of structural units II provided by the comonomer.

[0090] According to the present invention, the comonomer is selected from ethylene and α-olefins having 4 to 10 carbon atoms. Preferably, the comonomer is selected from at least one of ethylene, butene (such as 1-butene), pentene (such as 1-pentene), 4-methyl-1-pentene, hexene (such as 1-hexene), heptene (such as 1-heptene) and octene (such as 1-octene), more preferably ethylene and / or butene.

[0091] According to the present invention, the xylene solubles content of the heterophasic propylene copolymer is 0.5-40 wt%, preferably 0.6-35 wt%.

[0092] According to the present invention, the melt flow rate of the heterophasic propylene copolymer at 230°C and a load of 2.16 kg is 0.1 g / 10min-12 g / 10min, preferably 2 g / 10min-8 g / 10min;

[0093] According to the present invention, the molecular weight distribution of the heterophasic propylene copolymer is 4-10, preferably 3-8.

[0094] In the present invention, the propylene homopolymer and the heterophasic propylene copolymer are propylene homopolymers and heterophasic propylene copolymers prepared by catalysis with a Ziegler-Natta catalyst and / or a metallocene catalyst.

[0095] According to the present invention, the polypropylene composition further comprises at least one selected from the following components: ethylene vinyl acetate copolymer, ethylene methyl acrylate copolymer, polyolefin plastomer, polyolefin elastomer and polybutene.

[0096] According to the present invention, the antioxidant composite auxiliary agent comprises an antioxidant and an acid absorbent.

[0097] According to the present invention, the weight ratio of the antioxidant to the acid scavenger is 1-8:1, preferably 1-6:1.

[0098] According to the present invention, the antioxidant is selected from at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butyl)phenyl phosphite, octadecyl propionate and alkylated polyphenols.

[0099] According to the present invention, the acid absorber is a stearate, preferably at least one selected from calcium stearate, zinc stearate and sodium stearate.

[0100] According to the present invention, the antioxidant composite auxiliary agent is a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)trisphosphite and calcium stearate, wherein the weight ratio of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)trisphosphite to calcium stearate is (1-3):(1-3):1, preferably (2-3):(2-3):1.

[0101] According to the present invention, the polypropylene composition does not contain coupling agent and dispersant.

[0102] In the present invention, the polypropylene composition further comprises an α-crystalline nucleating agent and / or a β-crystalline nucleating agent.

[0103] In the present invention, the α-crystal nucleating agent is selected from at least one of substituted aromatic phosphate α-nucleating agents, dibenzylidene sorbitol α-nucleating agents, substituted aromatic carboxylate α-nucleating agents, and dehydroabietic acid soap α-nucleating agents; the β-crystal nucleating agent is selected from at least one of inorganic oxide β-nucleating agents, inorganic salt β-nucleating agents, condensed ring aromatic hydrocarbon β-nucleating agents, organic carboxylic acids and their salts β-nucleating agents, aromatic amide β-nucleating agents, and rare earth β-nucleating agents. There is no particular limitation on the amount of the α-crystal nucleating agent and / or the β-crystal nucleating agent, and it can be used according to the conventional amount in the art. For example, based on 100 parts by weight of polypropylene, the amount of the α-crystal nucleating agent and / or the β-crystal nucleating agent is 0.01-1 parts by weight.

[0104] According to the present invention, the polypropylene composition has hydrophilicity.

[0105] The second aspect of the present invention provides use of the polypropylene composition in a polyolefin microporous breathable film.

[0106] The third aspect of the present invention provides a method for preparing the above-mentioned polypropylene composition, characterized in that the method comprises:

[0107] (1) mixing polypropylene, a porogen and an antioxidant composite auxiliary agent to obtain a mixture;

[0108] (2) The mixture is melt-blended, extruded, pelletized and dried in a twin-screw extruder to obtain the polypropylene composition.

[0109] According to the present invention, the rotation speed of the twin-screw extruder is 100-400r / min.

[0110] According to the present invention, the temperatures of the feeding section, plasticizing section, homogenizing section and die of the twin-screw extruder are 150-180°C, 180-210°C, 185-225°C and 190-220°C respectively.

[0111] A fourth aspect of the present invention provides a polyolefin microporous breathable membrane, characterized in that the microporous breathable membrane is made from the above-mentioned polypropylene composition.

[0112] In the present invention, the polyolefin microporous breathable membrane prepared from the above polypropylene composition not only retains the excellent physical properties of the polypropylene composition, but more importantly, the polyolefin microporous breathable membrane has high air permeability and can be used in the fields of disposable medical and sanitary products, water-blocking and moisture-permeable materials, etc.

[0113] In the present invention, there is no particular limitation on the preparation method of the polyolefin microporous breathable film, and the film can be prepared according to conventional preparation methods in the art, for example, a polypropylene composition is added to an extrusion casting machine for melting and casting, the extrusion temperature is 210-250°C, the cooling roller temperature is 30-70°C, and a polypropylene cast film is prepared. The cast film sample is cut into a standard sample, and is placed in a stretching fixture of a film biaxial stretching tester for heating and stretching, the stretching temperature is 140-160°C, the stretching ratio is 3-7, and the stretched film is heat-set at 90-115°C for 5 minutes to obtain a polypropylene microporous film.

[0114] The present invention will be described in detail below by way of examples. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.

[0115] The relevant data in the present invention and its embodiments are obtained by the following test methods:

[0116] 1. The content of each structural unit in maleic anhydride copolymer microspheres is 1 H NMR was tested by 1 The content of each structural unit was calculated from the ratio of the peak area corresponding to the characteristic hydrogen in the corresponding structural unit in H NMR;

[0117] 2. Polymerization yield of maleic anhydride copolymer (Cp): Cp = Mp × 100% / Mm

[0118] Wherein, Mp is the mass of the obtained polymer; Mm is the total mass of the added monomers;

[0119] 3. Copolymer microsphere particle size test method: After the copolymer microsphere powder is vacuum sprayed with gold, the morphology is observed on a Hitachi S4800 field emission scanning electron microscope of Hitachi. 500 microspheres are selected from the electron microscope photos, and their diameters are measured. The average particle size of the microspheres is calculated by the mathematical average method.

[0120] 4. Conversion efficiency of mixed C4: weigh the polymer after the reaction, conversion efficiency (%) = [(4×actual mass of the obtained polymer) / (11×actual mass of C4 used)]×100%;

[0121] 5. The morphology of the cross section of the polypropylene composite sample and the dispersion of the porogen: The sample was soaked in liquid nitrogen for 15 minutes and then fractured. The cross section was treated with gold spraying. The cross section of the material was characterized by a Hitachi S4800 field emission scanning electron microscope to obtain a microscopic morphology photograph;

[0122] 6. Melt flow rate (MFR): measured at 230°C and 2.16 kg load according to the method specified in GB / T 3682-2000;

[0123] 7. Tensile properties: measured using a universal tensile testing machine in accordance with the method specified in GB / T 1040.3-2006.

[0124] 8. T C , Tm and △Hm: Differential scanning calorimeter was used to analyze the melting process and crystallization process of the material. The specific operation is: under nitrogen protection, 5-10 mg of sample was measured from 20℃ to 200℃ using a three-stage temperature rise and fall measurement method, and the change in heat flow reflects the melting and crystallization process of the material. The crystallization temperature T was calculated according to GB / T 19466.3-2004. C , melting temperature Tm and melting enthalpy △Hm.

[0125] 9. Contact angle test method: Use the EASY DROP contact angle tester from KRUSS Company of Germany with a measurement range of 1-180° and a resolution of 0.1°. Use the dynamic contact angle measurement mode. Each time, a fixed volume of 2 μL of deionized water is dropped on a sample formed by melting and hot pressing the polypropylene composition at 200°C. The calculated initial contact angle is taken as the contact angle measurement value of the sample. Perform 5 parallel measurements and calculate the average value.

[0126] 10. Air permeability: The Gurley value of the microporous membrane is measured using an air permeability meter. The Gurley value refers to the time required for a specific amount of air to pass through a microporous membrane of a specific area under a specific pressure. The smaller the Gurley value, the higher the air permeability. The measurement conditions are: working pressure 8.5 kPa, test area 645.2 mm 2 .

[0127] The raw materials used in the examples and comparative examples are all commercially available.

[0128] Preparation Example 1

[0129] Preparation of porogen A1

[0130] 342.6g of maleic anhydride, 62.5g of azobisisobutyronitrile, 311.5g of styrene, 1.387L of acetone and 4.75L of hexane (the amount of hexane is 77.4vol%) are added to a 20L reactor. After the materials are evenly mixed, nitrogen is passed through for 20 minutes, the reactor temperature is raised to 70°C, and the reaction is carried out for 6 hours. After the reaction is completed, the obtained polymer emulsion suspension is centrifuged at a speed of 2000rad / min for 20min by a centrifuge to obtain 582g of porogen maleic anhydride styrene copolymer microspheres A1, corresponding to a polymerization yield of 89%. In the polymerization monomer, the amount of maleic anhydride is 52.4wt%, the amount of styrene is 47.6wt%, the mass concentration of maleic anhydride and comonomer in the homogeneous solution is 13.2wt%, and the mass concentration of initiator is 1.26wt%.

[0131] The polymer microspheres 1 According to H NMR measurement, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 49%, and the molar content of the structural unit B derived from styrene was 51%.

[0132] The average particle size of the porogen maleic anhydride copolymer microspheres A1 is about 1000 nm.

[0133] Preparation Example 2

[0134] The mass percentage of each component in the mixed C4 is as follows: 1,3-butadiene, 0.06%; trans-2-butene, 12.67%; isobutane, 37.09%; isobutylene, 19.48%; cis-2-butene, 27.79%; 1-butene, 1.02%; others, 1.89%. 17.5 kg of the mixed C4 composed above is introduced into a 200 L reactor containing 14.5 kg of maleic anhydride, 4.1 kg of dibenzoyl peroxide and 120 L of isoamyl acetate organic reaction liquid for free radical copolymerization. The copolymerization pressure is 1 MPa, the copolymerization temperature is 80 ° C, and the copolymerization time is 6 hours; the weight ratio of maleic anhydride to mixed C4 is 1:1.21. The concentration of maleic anhydride in the organic solvent is 12.1 wt%.

[0135] The copolymerization product was passed into a flash separator for gas-liquid separation at 30°C and 0MPa, and the obtained liquid-solid mixture was further centrifuged in a centrifugal separator at 4000rad / min for 20min to obtain a solid product, and the liquid was returned to the reactor. The solid product was then washed with hexane, and the filter cake obtained by filtration through a sand core funnel was vacuum dried at 90°C for 8h to obtain 24.5kg of maleic anhydride-mixed C4 copolymer A2.

[0136] The porogen maleic anhydride-mixed C4 copolymer A2 was 1According to H NMR measurement, based on the total molar amount of each structural unit in the polymer, the molar content of structural unit A derived from maleic anhydride is 49 mol%, and the molar content of structural unit B derived from mixed C4 is 51 mol%. The conversion efficiency of mixed C4 calculated by weight method is 51 wt%.

[0137] The average particle size of maleic anhydride-mixed C4 copolymer microspheres is about 1220 nm.

[0138] Preparation Example 3

[0139] Preparation of porogen A3

[0140] 415.1g maleic anhydride, 55.5g azobisisobutyronitrile, 277.5g styrene, 1.198L acetone and 4.75L hexane (the amount of hexane is 79.9vol%) are added to a 20L reactor. After the materials are evenly mixed, nitrogen is passed through for 20min, the reactor temperature is raised to 70°C, and the reaction is carried out for 5h. After the reaction is completed, the obtained polymer emulsion suspension is centrifuged at a speed of 2000rad / min for 20min to obtain 554g of polymer microspheres A2, corresponding to a polymerization yield of 80%. In the polymerization monomer, the amount of maleic anhydride is 59.9wt%, the amount of styrene is 40.1wt%, the mass concentration of maleic anhydride and comonomer in the homogeneous solution is 14.3wt%, and the mass concentration of initiator is 1.15wt%.

[0141] The polymer microspheres 1 According to H NMR measurement, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 49%, and the molar content of the structural unit B derived from styrene was 51%.

[0142] The average particle size of the porogen maleic anhydride copolymer microspheres A2 is about 1200 nm.

[0143] Preparation Example 4

[0144] Preparation of porogen

[0145] 295.5g maleic anhydride, 62.5g azobisisobutyronitrile, 278.8g styrene, 1.453L acetone and 4.75L hexane (the amount of hexane is 76.6vol%) are added to a 20L reactor. After the materials are evenly mixed, nitrogen is passed through for 20 minutes, the reactor temperature is raised to 70°C, and the reaction is carried out for 5h. After the reaction is completed, the obtained polymer emulsion suspension is centrifuged at a speed of 2000rad / min for 20min by a centrifuge to obtain 505g of porogen maleic anhydride styrene copolymer microspheres A1, corresponding to a polymerization yield of 88%. In the polymerization monomer, the amount of maleic anhydride is 51.5wt%, the amount of styrene is 48.5wt%, and in the homogeneous solution, the mass concentration of maleic anhydride and comonomer is 11.7wt%, and the mass concentration of initiator is 1.27wt%.

[0146] The polymer microspheres 1 According to H NMR measurement, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 50%, and the molar content of the structural unit B derived from styrene was 50%.

[0147] The average particle size of the porogen maleic anhydride copolymer microspheres A4 is about 700 nm.

[0148] Preparation Example 5

[0149] Preparation of porogen

[0150] 145.5g maleic anhydride, 62.5g azobisisobutyronitrile, 167.8g styrene, 2.265L acetone and 2.875L hexane (the amount of hexane is 55.9vol%) are added to a 20L reactor. After the materials are evenly mixed, nitrogen is passed through for 20 minutes, the reactor temperature is raised to 70°C, and the reaction is carried out for 5 hours. After the reaction is completed, the obtained polymer emulsion suspension is centrifuged at a speed of 2000rad / min for 20 minutes by a centrifuge to obtain 232g of porogen maleic anhydride styrene copolymer microspheres A1, corresponding to a polymerization yield of 74%. In the polymerization monomer, the amount of maleic anhydride is 46.4wt%, the amount of styrene is 53.6wt%, the mass concentration of maleic anhydride and comonomer in the homogeneous solution is 7.7wt%, and the mass concentration of initiator is 1.54wt%.

[0151] The polymer microspheres 1 According to H NMR measurement, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 47%, and the molar content of the structural unit B derived from styrene was 53%.

[0152] The average particle size of the porogen maleic anhydride copolymer microspheres A4 is about 450 nm.

[0153] Example 1

[0154] Preparation of polypropylene composition

[0155] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 100 parts of porogen A1 and 1 part of antioxidant composite auxiliary in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0156] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1. The polypropylene composition was melted and pressed into sheets at 200° C., and the thickness of the sample sheet was 120-160 μm. Figure 1 is a SEM photo of the cross section of a polypropylene composite sample. Figure 1 It can be seen that the porogen particle size is uniform and evenly distributed in the polypropylene matrix.

[0157] Example 2

[0158] Preparation of polypropylene composition

[0159] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 70 parts of porogen A1 and 1 part of antioxidant composite auxiliary in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0160] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1. The polypropylene composition was melted and pressed into sheets at 200° C., and the thickness of the sample sheet was 120-160 μm. Figure 2 is a SEM photo of the cross section of a polypropylene composite sample. Figure 2It can be seen that the porogen particle size is uniform and evenly distributed in the polypropylene matrix.

[0161] Example 3

[0162] Preparation of polypropylene composition

[0163] 90 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9), 10 parts of heterophasic propylene copolymer (MFR of 1.8 g / 10 min, ethylene content of 13.2%, xylene soluble content of 31.4%, molecular weight distribution of 3.9) are blended with 85 parts of porogen A1 and 1 part of antioxidant composite auxiliary in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0164] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1. The polypropylene composition was melted and pressed into sheets at 200° C., and the thickness of the sample sheet was 120-160 μm. Figure 3 is a SEM photo of the cross section of a polypropylene composite sample. Figure 3 It can be seen that the porogen particle size is uniform and evenly distributed in the polypropylene matrix.

[0165] Example 4

[0166] Preparation of polypropylene composition

[0167] 70 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9), 30 parts of heterophasic propylene copolymer (MFR of 2.8 g / 10 min, butene content of 1.1 mol%, xylene soluble content of 3.3%, molecular weight distribution of 4.5) are blended with 65 parts of porogen A2 and 1 part of antioxidant composite auxiliary in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0168] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1.

[0169] Example 5

[0170] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 110 parts of porogen A3 and 1 part of antioxidant composite auxiliary in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0171] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1. The polypropylene composition was melted and pressed into sheets at 200° C., and the thickness of the sample sheet was 120-160 μm. Figure 4 is a SEM photo of the cross section of a polypropylene composite sample. Figure 4 It can be seen that the porogen particle size is uniform and evenly distributed in the polypropylene matrix.

[0172] Example 6

[0173] Preparation of polypropylene composition

[0174] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 110 parts of porogen A4 and 1 part of antioxidant composite auxiliary in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0175] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1.

[0176] Comparative Example 1

[0177] Preparation of polypropylene composition

[0178] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 25 parts of porogen A1 and 1 part of antioxidant composite auxiliary in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0179] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1. The polypropylene composition was melted and pressed into sheets at 200° C., and the thickness of the sample sheet was 120-160 μm. Figure 5 is a SEM photo of the cross section of a polypropylene composite sample. Figure 5 It can be seen that the porogen particle size is uniform, but the number is small and the distribution is uneven.

[0180] Comparative Example 2

[0181] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%; xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 100 parts of nano-CaCO3 powder (Shanghai Yuanjiang Chemical Co., Ltd., 10000 mesh) and 1 part of antioxidant composite auxiliary agent in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0182] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1. The polypropylene composition was melted and pressed into sheets at 200° C., and the thickness of the sample sheet was 120-160 μm. Figure 6 is a SEM photo of the cross section of a polypropylene composite sample. Figure 6 It can be seen that the porogen is obviously agglomerated.

[0183] Comparative Example 3

[0184] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%; xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 110 parts of nano BaSO4 powder (Sahliben Blanc Fixe Micro, organically coated, d50=0.7 μm) and 1 part of antioxidant composite auxiliary agent in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0185] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1. The polypropylene composition was melted and pressed into sheets at 200° C., and the thickness of the sample sheet was 120-160 μm. Figure 7 is a SEM photo of a polypropylene composite sample. Figure 7 It can be seen that the porogen is obviously agglomerated.

[0186] Comparative Example 4

[0187] Preparation of polypropylene composition

[0188] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 140 parts of porogen A1 and 1 part of antioxidant composite auxiliary in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0189] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1.

[0190] Comparative Example 5

[0191] Preparation of polypropylene composition

[0192] 100 parts of propylene homopolymer (MFR of 3.5 g / 10 min, isotacticity of 98.4%, xylene soluble content of 3.1%, molecular weight distribution of 4.9) are blended with 100 parts of porogen A5 and 1 part of antioxidant composite auxiliary agent in a high-speed mixer, wherein the antioxidant is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0193] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 250 r / min, and the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder were 175° C., 195° C., 210° C. and 200° C., respectively; the polypropylene composition of the present invention was obtained. The obtained polypropylene composition was dried at 80° C. for 12 hours. The properties of the polypropylene composition are shown in Table 1.

[0194] Table 1

[0195]

[0196]

[0197] It can be seen from Table 1 that the melt flow rate (MFR) of the polypropylene composition provided by the present invention meets the requirements of the casting process, and ΔH mPP With △H m组合物 When the difference meets the range of the present invention, it indicates that the maleic anhydride copolymer microspheres in the composition are evenly distributed in the composition, and the material has good mechanical properties and hydrophilicity, and can meet the requirements of the stretching ratio of the breathable film.

[0198] Test Case

[0199] The polypropylene composition of the embodiment and the preparation example is added to an extrusion casting machine for melting and casting, the extrusion temperature is 210-250°C, the cooling roller temperature is 30-70°C, and a polypropylene cast film is prepared. The cast film sample is cut into a standard sample, and placed in the stretching fixture of a film biaxial stretching tester for heating and stretching, the stretching temperature is 140-160°C, the stretching ratio is 3-7, and the stretched film is heat-set at 90-115°C for 5 minutes to obtain a polypropylene microporous film. The properties of the polypropylene microporous breathable film are shown in Table 2.

[0200] Table 2

[0201]

[0202]

[0203] As can be seen from Table 2, the present invention significantly improves the uniformity of the dispersion of the porogen in the matrix resin without using a coupling agent and a dispersant by reasonably selecting an organic porogen with uniform particles and a polyolefin matrix resin, and improves the mechanical properties and air permeability of the polyolefin resin for the breathable membrane to a certain extent. The present invention adopts a simple process route to obtain a polypropylene composition for a breathable membrane with uniform pore size distribution. The composition has a certain hydrophilicity, can give full play to the role of the porogen, can be used to prepare a microporous breathable membrane, and is widely used in the fields of disposable medical and sanitary products, waterproof and breathable materials, etc.

[0204] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A polypropylene composition, characterized in that The composition comprises polypropylene, a pore-forming agent and an antioxidant composite auxiliary agent; Based on 100 parts by weight of polypropylene, the amount of the porogen is 50-120 parts by weight, and the amount of the antioxidant composite auxiliary is 0.1-2 parts by weight; The porogen is maleic anhydride copolymer microspheres, and the average particle size of the maleic anhydride copolymer microspheres is 500-1600nm; The copolymer in the maleic anhydride copolymer microspheres comprises a structural unit A derived from maleic anhydride and a structural unit B derived from a comonomer, and based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 48-55%, and the molar content of the structural unit B is 45-52%; The comonomer is selected from at least one of styrene, α-methylstyrene, vinyl acetate, C4 olefins and C5 olefins.

2. The polypropylene composition according to claim 1, wherein Based on 100 parts by weight of polypropylene, the amount of the porogen is 60-110 parts by weight, and the amount of the antioxidant composite auxiliary is 0.2-1.8 parts by weight; And / or, the average particle size of the maleic anhydride copolymer microspheres is 600-1300 nm.

3. The polypropylene composition according to claim 1 or 2, wherein The melting enthalpy of the polypropylene is ΔH mPP , the melting enthalpy of the polypropylene composition is ΔH m组合物 ; Among them, △H mPP With △H m组合物 The difference is 15-38 J / g.

4. The polypropylene composition according to claim 3, wherein △H mPP With △H m组合物 The difference is 18-32 J / g.

5. The polypropylene composition according to any one of claims 1 to 2 and 4, wherein: Based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 49-51%, and the molar content of the structural unit B is 49-51%.

6. The polypropylene composition according to any one of claims 1 to 2 and 3, wherein: The porogen is prepared according to the following steps: (1) dissolving maleic anhydride, comonomer and initiator in a reaction medium in an inert atmosphere to form a homogeneous solution; (2) the homogeneous solution is subjected to a polymerization reaction to obtain a copolymer emulsion suspension, and then the porogen is obtained after solid-liquid separation; Wherein, based on the total weight of maleic anhydride and the comonomer, the amount of maleic anhydride is 50-90wt%, and the amount of the comonomer is 10-50wt%; The reaction medium is a mixture of the compound represented by formula (1) and an alkane; Wherein, R1 and R2 are each independently an alkyl group having 1 to 6 carbon atoms.

7. The polypropylene composition according to claim 6, wherein The comonomer is selected from at least one of styrene, α-methylstyrene and vinyl acetate.

8. The polypropylene composition according to claim 6, wherein Based on the total weight of the homogeneous solution, the total mass concentration of the maleic anhydride and the comonomer is 5-25wt%; And / or, based on the total weight of the homogeneous solution, the mass concentration of the initiator is 0.01-5wt%.

9. The polypropylene composition according to claim 8, wherein Based on the total weight of the homogeneous solution, the total mass concentration of the maleic anhydride and the comonomer is 5-20wt%; And / or, based on the total weight of the homogeneous solution, the mass concentration of the initiator is 1-4 wt %.

10. The polypropylene composition according to claim 7, wherein Based on the total weight of maleic anhydride and the comonomer, the amount of maleic anhydride used is 50-60wt%, and the amount of styrene used is 40-50wt%.

11. The polypropylene composition according to claim 6, wherein In formula (1), R1 and R2 are each independently methyl or ethyl; and / or, the alkane is an alkane having 6 to 12 carbon atoms; And / or, the alkane is used in an amount of 50-90 vol% based on the total volume of the reaction medium.

12. The polypropylene composition according to claim 11, wherein The alkane is used in an amount of 60-80 vol% based on the total volume of the reaction medium.

13. The polypropylene composition according to claim 6, wherein The polymerization reaction conditions include: polymerization temperature of 61-100° C., and polymerization time of 1-24 h.

14. The polypropylene composition according to claim 13, wherein The polymerization reaction conditions include: polymerization temperature of 70-90° C., and polymerization time of 2-12 h.

15. The polypropylene composition according to claim 1 or 2, wherein: The preparation method of the porogen comprises the following steps: In the presence of an inert atmosphere, an initiator and an organic solvent, maleic anhydride and a comonomer are copolymerized to obtain the maleic anhydride copolymer microspheres.

16. The polypropylene composition according to claim 15, wherein The comonomer is selected from mixed C4 and / or mixed C5; and / or, the weight ratio of the maleic anhydride to the comonomer is 1:(0.2-3); and / or, based on the total weight of the maleic anhydride, the amount of the initiator is 0.05-20 mol%; And / or, the organic solvent is selected from at least one of isoamyl acetate, butyl acetate, isopropyl acetate and ethyl acetate; And / or, based on the total weight of the organic solvent, the concentration of the maleic anhydride is 5-25 wt %.

17. The polypropylene composition according to claim 16, wherein The weight ratio of the maleic anhydride to the comonomer is 1:(0.8-3); And / or, based on the total weight of the organic solvent, the concentration of the maleic anhydride is 10-20 wt %.

18. The polypropylene composition according to claim 15, wherein The copolymerization reaction conditions include: copolymerization reaction temperature of 50-100° C., copolymerization reaction pressure of 0.2-2 MPa, and copolymerization reaction time of 5-10 h.

19. The polypropylene composition according to claim 18, wherein The copolymerization reaction conditions include: copolymerization reaction temperature of 70-90° C., copolymerization reaction pressure of 0.5-1 MPa, and copolymerization reaction time of 6-9 h.

20. The polypropylene composition according to any one of claims 1 to 2, 4, 7 to 14, 16 to 19, wherein: The polypropylene is a propylene homopolymer or a mixture of a propylene homopolymer and a heterophasic propylene copolymer.

21. The polypropylene composition according to claim 20, wherein Based on 100 parts by weight of polypropylene, the amount of the propylene homopolymer is 60-95 parts by weight, and the amount of the heterophasic propylene copolymer is 5-40 parts by weight.

22. The polypropylene composition according to claim 21, wherein Based on 100 parts by weight of polypropylene, the amount of the propylene homopolymer is 70-95 parts by weight, and the amount of the heterophasic propylene copolymer is 5-30 parts by weight.

23. The polypropylene composition according to claim 20, wherein The isotacticity of the propylene homopolymer is 95-99.5%; and / or, the xylene soluble content of the propylene homopolymer is 0.3-5wt%; and / or, the propylene homopolymer has a melt flow rate of 0.5 g / 10 min to 10 g / 10 min at 230° C. and a load of 2.16 kg; And / or, the molecular weight distribution of the propylene homopolymer is 1-10.

24. The polypropylene composition according to claim 23, wherein The isotacticity of the propylene homopolymer is 96-99.5%; and / or, the xylene soluble content of the propylene homopolymer is 0.5-4wt%; and / or, the propylene homopolymer has a melt flow rate of 2 g / 10 min to 6 g / 10 min at 230° C. and a load of 2.16 kg; And / or, the molecular weight distribution of the propylene homopolymer is 2-6.

25. The polypropylene composition according to claim 20, wherein The heterophasic propylene copolymer contains 60-99 wt% of structural units I provided by propylene and 1-40 wt% of structural units II provided by comonomer N; and / or, the heterophasic propylene copolymer has a xylene soluble content of 0.5-40 wt%; and / or, the heterophasic propylene copolymer has a melt flow rate at 230° C. and 2.16 kg load of 0.1 g / 10 min to 12 g / 10 min; And / or, the molecular weight distribution of the heterophasic propylene copolymer is 4-10.

26. The polypropylene composition according to claim 25, wherein The xylene soluble content of the heterophasic propylene copolymer is 0.6-35 wt%; and / or, the heterophasic propylene copolymer has a melt flow rate at 230° C. and 2.16 kg load of 2 g / 10 min to 8 g / 10 min; And / or, the molecular weight distribution of the heterophasic propylene copolymer is 3-8.

27. The polypropylene composition according to claim 25, wherein The comonomer N is selected from at least one of ethylene, butene, pentene, 4-methyl-1-pentene, hexene, heptene and octene.

28. The polypropylene composition according to claim 27, wherein The comonomer N is ethylene and / or butene.

29. The polypropylene composition according to claim 20, wherein The polypropylene composition further comprises at least one selected from the group consisting of ethylene vinyl acetate copolymer, ethylene methyl acrylate copolymer, polyolefin plastomer, polyolefin elastomer and polybutene.

30. The polypropylene composition according to any one of claims 1 to 2, 4, 7 to 14, 16 to 19, 21 to 29, wherein: The antioxidant composite auxiliary agent comprises an antioxidant and an acid absorbent.

31. The polypropylene composition according to claim 30, wherein The weight ratio of the antioxidant to the acid scavenger is 1-8:1; and / or, the antioxidant is at least one selected from pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butyl)phenyl phosphite, octadecyl propionate and alkylated polyphenols; And / or, the acid scavenger is a stearate.

32. The polypropylene composition according to claim 31, wherein The acid absorber is selected from at least one of calcium stearate, zinc stearate and sodium stearate.

33. The polypropylene composition according to claim 31, wherein The antioxidant composite auxiliary agent is a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)trisphosphite and calcium stearate, wherein the weight ratio of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)trisphosphite to calcium stearate is (1-3):(1-3):

1.

34. The polypropylene composition according to any one of claims 1-2, 4, 7-14, 16-19, 21-29, 31-33, wherein The polypropylene composition does not contain coupling agent and dispersant.

35. The polypropylene composition according to any one of claims 1-2, 4, 7-14, 16-19, 21-29, 31-33, wherein The polypropylene composition has hydrophilicity.

36. Use of the polypropylene composition according to any one of claims 1 to 35 in a polyolefin microporous breathable film.

37. A method for preparing the polypropylene composition according to any one of claims 1 to 35, characterized in that: The method comprises: (1) mixing polypropylene, a porogen and an antioxidant composite auxiliary agent to obtain a mixture; (2) The mixture is melt-blended, extruded, pelletized and dried in a twin-screw extruder to obtain the polypropylene composition.

38. The preparation method according to claim 37, wherein: The speed of the twin-screw extruder is 100-400r / min; And / or, the feeding section, plasticizing section, homogenizing section and die temperature of the twin-screw extruder are 150-180°C, 180-210°C, 185-225°C, 190-220°C respectively.

39. A polyolefin microporous breathable membrane, characterized in that: The polyolefin microporous breathable membrane is made from the polypropylene composition described in any one of claims 1-35.

Citation Information

Cited By

  • Resin composition comprising fiber material and secondary battery container for electric vehicles using same

    WO2026105939A1