A method for producing light white oil and / or industrial white oil
By using alumina-containing support and non-precious metal catalysts in the production of light white oil and industrial white oil, the problems of long processes, high costs and insufficient aromatic content in the prior art are solved, and high efficiency and low quality are achieved Cost white oil production meets the light white oil standards.
Patent Information
- Application Number
- CN202111273193.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The existing production methods for lightweight white oil and industrial white oil have problems such as long process, high cost, complex operation and the aromatic content cannot meet the standards.
Using hydrotreatment methods containing alumina support and non-precious metal catalysts, hydrotreatment and hydrofining treatment in the presence of hydrogen, reduce sulfur, nitrogen and aromatic content through appropriate acidic catalysts, avoid cracking reactions, and satisfy light white Oil standard.
The process flow is simplified, the cost is reduced, the product yield is improved, and the aromatic content is significantly reduced, meeting the requirements of light white oil standards.
Smart Images

Figure CN116064150B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing light white oil and / or industrial white oil. Background Art
[0002] White oil is a kind of ultra-deeply refined mineral oil, mainly composed of paraffins and cycloalkanes, and almost no aromatics. Because it is colorless, tasteless, odorless and chemically inert, and exhibits excellent light and thermal stability, it is widely used in the fields of chemical industry, food, medicine, daily chemicals, etc. Traditionally speaking, white oil belongs to the lubricating oil fraction >350℃, but with the emergence of new industries using white oil, the distillation range of white oil has been greatly expanded, and the fractions above 120℃ can produce white oil products.
[0003] In addition to meeting the functional indicators of white oil, impurities such as S and N in the raw materials must be deeply removed during its production process, and aromatics must be highly saturated, so that the product meets the safety indicators for use. In recent years, hydrogenation technology has been widely used in the field of white oil production. In the presence of hydrogen and catalysts, aromatics in the raw materials can be deeply hydrogenated and saturated, and non-ideal components can be converted into qualified products, with the characteristics of good product quality, stable production process, and high product yield.
[0004] CN107937024A discloses a method for producing high-quality light white oil from base oil. The method comprises the following steps: heating the raw base oil to a reaction temperature, fully mixing it with hydrogen, and then feeding it into a hydrogenation reactor carrying a catalyst I. Under the action of the hydrogenation refining catalyst I, a hydrogenation refining reaction is performed to remove most of the S, N and aromatic impurities in the raw base oil; the product after the reaction enters two reactors respectively carrying catalysts II and III in series and contacts with the catalysts II and III to perform S removal and aromatic saturation reactions; the obtained reactants are separated into gas and liquid by high and low pressure separators and then enter a fractionation system for fine cutting to obtain a variety of high-quality light white oil products with different registration numbers. However, the acidity of catalysts II and III used in this method is relatively strong. In the process of further desulfurization and aromatic saturation reaction of the refined raw materials, a relatively obvious cracking reaction occurred, resulting in some light oil and "1# light white oil" with a final boiling point of <120°C, which does not meet the technical standard of NB / SH / T 0913-2015 "Light White Oil" (hereinafter referred to as "Light White Oil Standard"). Moreover, the three reactors in series make the process too long and the investment high.
[0005] Patent CN 103059974B discloses a hydrogenation process for producing food-grade solvent oil, patent CN103059975B discloses a hydrogenation process for producing solvent oil flexibly, and patent CN103666554B discloses a hydrogenation process for producing high-quality solvent oil. The above methods can produce high-quality solvent products with a sulfur content of <0.5μg / g and an aromatic content of <100μg / g from kerosene or light diesel fractions. However, both methods use a two-stage dearomatization process using a non-precious metal catalyst and a precious metal catalyst, and require a separation device to be set between the reactors or a countercurrent contact reaction to be performed in the precious metal catalyst reaction zone, which has the problems of high catalyst cost, long process, and complicated operation.
[0006] CN1190474C discloses a method for producing kerosene type solvent oil and its catalyst. The method uses straight run kerosene or hydrocracking kerosene fraction at 130℃~300℃ as raw material, and adopts W-Ni / TiO2-Al2O3 or W-Mo-Ni / TiO2-Al2O3 as catalyst to produce high quality kerosene type solvent oil. CN100513530C discloses a method for hydrogenation and reforming of solvent oil. The method uses petroleum fraction containing one or several fractions of gasoline, kerosene and diesel as raw material, and reacts with a hydrogenation and reforming catalyst containing β zeolite in the presence of hydrogen and under suitable conditions to produce solvent oil with excellent performance. However, the aromatic content of the product obtained by the above method cannot meet the requirements of "light white oil II" for aromatic content in the light white oil standard. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of the existing methods for producing light white oil and / or industrial white oil, such as long process, high cost, complicated operation, low yield, high aromatic content in the white oil products, and to provide a method for producing light white oil and / or industrial white oil.
[0008] In order to achieve the above object, the present invention provides a method for producing light white oil and / or industrial white oil, the method comprising:
[0009] S1. In the presence of hydrogen, the feedstock oil is contacted with a hydroprocessing catalyst for hydroprocessing to obtain a hydroprocessing product; the feedstock oil contains a straight-run kerosene fraction and / or a straight-run diesel fraction;
[0010] S2. In the presence of hydrogen, contacting the hydrotreated product with a hydrorefining catalyst for hydrorefining treatment to obtain a hydrorefined oil;
[0011] S3, separating the hydrorefined oil;
[0012] The hydroprocessing catalyst contains an alumina carrier and a first hydrogenation active component, the alumina carrier contains fluorine, and the ratio of B acid to L acid of pyridine infrared measured at 200° C. of the alumina carrier is 0.15-1.45.
[0013] Optionally, the ratio of B acid to L acid of pyridine infrared measured at 200° C. of the alumina carrier is 0.16-1.35.
[0014] Optionally, the hydroprocessing catalyst is a non-precious metal catalyst; the first hydrogenation active component is a VIB group metal and / or a VIII group metal; preferably, the first hydrogenation active component is selected from one or more of Co, Ni, Mo and W;
[0015] Based on the dry weight of the hydroprocessing catalyst, the content of the first hydrogenation active component is 1-34% by weight in terms of oxide.
[0016] Optionally, the fluorine content is 0.01-6 wt % based on the dry weight of the hydroprocessing catalyst.
[0017] Optionally, in step S1, the conditions of the hydrotreatment include: hydrogen partial pressure of 1-20 MPa, temperature of 260-400°C, volume space velocity of 0.3-10 h -1 , the volume ratio of hydrogen to oil is (100-3000):1;
[0018] Preferably, the hydrogen partial pressure is 12-18 MPa, the temperature is 280-360°C, and the volume space velocity is 0.5-8h -1 , the volume ratio of hydrogen to oil is (300-1000):1.
[0019] Optionally, in step S2, the conditions of the hydrofining treatment include: hydrogen partial pressure of 1-20 MPa, temperature of 240-400°C, volume space velocity of 0.3-10 h -1 , the volume ratio of hydrogen to oil is (100-3000):1;
[0020] Preferably, the hydrogen partial pressure is 12-18 MPa, the temperature is 260-320°C, and the volume space velocity is 0.5-8 h -1 , the volume ratio of hydrogen to oil is (300-1000):1.
[0021] Optionally, the distillation range of the feedstock oil is 120-400°C and the pour point is -50°C to -6°C.
[0022] Optionally, the method comprises: contacting the feedstock oil with the hydrotreating catalyst in a hydrotreating reaction zone to perform the hydrotreating; and then contacting the obtained hydrotreating product with the hydrotreating catalyst in a hydrotreating reaction zone to perform the hydrotreating.
[0023] Optionally, the feedstock oil contains a straight-run kerosene fraction and a straight-run diesel fraction, and the straight-run kerosene fraction and the straight-run diesel fraction are alternately fed into the hydroprocessing reaction zone in a switching feed manner.
[0024] Optionally, in step S3, the separation includes: distilling the hydrorefined oil to obtain light white oil and / or industrial white oil.
[0025] Optionally, the hydrotreating catalyst is a non-precious metal catalyst;
[0026] The hydrotreating catalyst contains a second hydrogenation active component and an inert carrier;
[0027] The inert carrier includes one or more of silicon oxide, aluminum oxide, titanium oxide and magnesium oxide; the second hydrogenation active component is selected from one or more of nickel, molybdenum, tungsten and cobalt.
[0028] Compared with the prior art, the method provided by the present invention for producing light white oil and / or industrial white oil has the following obvious advantages:
[0029] (1) The method of the present invention uses a hydroprocessing catalyst containing a fluorine-containing aluminum oxide carrier with suitable acidity, which can achieve deep desulfurization and denitrification of the raw oil while moderately opening and saturating the polycyclic aromatic hydrocarbons, thereby significantly reducing the sulfur, nitrogen, and aromatic hydrocarbon (especially polycyclic aromatic hydrocarbon) contents of the hydroprocessed oil and avoiding the occurrence of cracking reactions. The final product can meet the requirements of "light white oil II" in the light white oil standard for aromatic hydrocarbon content and has a high yield;
[0030] (2) The hydroprocessing catalyst and hydrofining catalyst used in this method are both non-precious metal catalysts, and there is no need to set up a gas stripping tower between different reaction zones. This method has the characteristics of small investment, simple process and easy operation.
[0031] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present invention. In the accompanying drawings:
[0033] Figure 1It is a process flow diagram of a specific implementation mode of the present invention. DETAILED DESCRIPTION
[0034] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0035] The present invention provides a method for producing light white oil and / or industrial white oil, the method comprising:
[0036] S1. In the presence of hydrogen, the feedstock oil is contacted with a hydroprocessing catalyst for hydroprocessing to obtain a hydroprocessing product; the feedstock oil contains a straight-run kerosene fraction and / or a straight-run diesel fraction;
[0037] S2. In the presence of hydrogen, contacting the hydrotreated product with a hydrorefining catalyst for hydrorefining treatment to obtain a hydrorefined oil;
[0038] S3, separating the hydrorefined oil;
[0039] The hydroprocessing catalyst contains an alumina carrier and a first hydrogenation active component, the alumina carrier contains fluorine, and the ratio of B acid to L acid of pyridine infrared measured at 200° C. of the alumina carrier is 0.15-1.45.
[0040] The hydroprocessing catalyst used in the method of the present invention is a chlorine-containing non-precious metal catalyst with suitable acidity, which can effectively reduce the sulfur, nitrogen and aromatic content in the hydroprocessing product, so that the final product can meet the requirements of "light white oil II" in the light white oil standard for aromatic content and has a high yield. At the same time, the hydrorefining catalyst is also a non-precious metal catalyst, which realizes that no precious metal catalyst is used in the reaction, thereby avoiding the need to set a gas stripping tower between different reaction zones, simplifying the process flow and operation.
[0041] In a preferred embodiment of the present invention, the ratio of B acid to L acid of pyridine infrared measured on an alumina carrier at 200° C. is 0.16-1.35, preferably 0.16-0.5, which can further improve the yield of white oil and reduce the content of white oil aromatics.
[0042] According to the present invention, the hydroprocessing catalyst can be commercially available or prepared by a method of the prior art, and the present invention does not impose specific restrictions on this. In a specific embodiment, the hydroprocessing catalyst is a non-precious metal catalyst; the first hydrogenation active component is a metal of Group VIB and / or a metal of Group VIII; preferably, the first hydrogenation active component is selected from one or more of Co, Ni, Mo and W; based on the dry weight of the hydroprocessing catalyst, the content of the first hydrogenation active component in terms of oxide can vary in a large range, for example, 1-34% by weight, preferably 5-25% by weight. The present application does not impose any restrictions on the preparation method of the hydroprocessing catalyst, which can be a method well known to those skilled in the art.
[0043] According to the present invention, the fluorine content can vary within a wide range, for example, 0.01-6 wt %, preferably 0.5-5 wt %, based on the dry weight of the hydroprocessing catalyst.
[0044] In a specific embodiment of the present invention, in step S1, the conditions of the hydrotreatment include: hydrogen partial pressure of 1-20 MPa, temperature of 260-400°C, volume space velocity of 0.3-10 h -1 , the volume ratio of hydrogen to oil is (100-3000):1; preferably, the pressure is 12-18MPa, the temperature is 280-360℃, and the volume space velocity is 0.5-8h -1 , the volume ratio of hydrogen to oil is (300-1000):1.
[0045] In a specific embodiment of the present invention, in step S2, the conditions of the hydrofining treatment include: hydrogen partial pressure of 1-20 MPa, temperature of 240-400°C, volume space velocity of 0.3-10 h -1 , the volume ratio of hydrogen to oil is (100-3000):1; preferably, the pressure is 12-18MPa, the temperature is 260-320℃, and the volume space velocity is 0.5-8h -1 , the volume ratio of hydrogen to oil is (300-1000):1.
[0046] In the present invention, the distillation range of the feedstock oil may be 120-400°C, and the pour point may be -50°C to -6°C, preferably, the distillation range is 155-350°C, and the pour point is -42°C to -12°C. When the method of the present invention uses the feedstock oil with the above characteristics to produce white oil, the quality and yield of the white oil product can be further improved.
[0047] In a specific embodiment of the present invention, the method comprises: contacting the feedstock oil with the hydroprocessing catalyst in a hydroprocessing reaction zone to perform the hydroprocessing; and then contacting the obtained hydroprocessing product with the hydroprocessing catalyst in a hydrofining reaction zone to perform the hydrofining treatment. In the above embodiment, the hydroprocessed product is directly subjected to the hydrofining treatment without providing a separation device between reactors or performing a countercurrent contact reaction in a noble metal catalyst reaction zone, so the process flow is short and the process operation is simple.
[0048] In a specific embodiment of the present invention, the raw oil contains a straight-run kerosene fraction and a straight-run diesel fraction. Preferably, the raw oil is pre-fractionated to obtain a straight-run kerosene fraction and a straight-run diesel fraction, and the straight-run kerosene fraction and the straight-run diesel fraction are alternately fed into the hydroprocessing reaction zone in a switching feed manner to adjust the reaction operating conditions according to different raw material properties, so that the hydrogenation reaction process is more sufficient, which is beneficial to further improve the yield and quality of the white oil product.
[0049] According to the present invention, in step S3, the separation includes: distilling the hydrorefined oil to obtain light white oil and / or industrial white oil. Distillation is an operation well known to those skilled in the art, such as flash distillation, precision distillation, atmospheric distillation, and vacuum distillation, as long as the light white oil and / or industrial white oil in the hydrorefined oil can be separated.
[0050] According to the present invention, the hydrorefining catalyst can be used to further remove sulfur and nitrogen, and deeply saturate aromatics, thereby improving the odor, color, thermal oxidation stability and other indicators of the oil product, so that the final products can meet the quality standards of "light white oil II" and industrial white oil in the light white oil standard. The hydrorefining catalyst can be selected from any catalyst in the prior art that can achieve this function, and can be a commercially available product or prepared by any existing method. For example, the hydrorefining catalyst of the present invention can be prepared by the method described in patent CN 1840618A, patent CN 1133723C, patent CN 1648214A and CN 1626279A. In a specific embodiment, the hydrorefining catalyst can be a non-precious metal catalyst; the hydrorefining catalyst contains a second hydrogenation active component and an inert carrier; the inert carrier includes one or more of silicon oxide, aluminum oxide, titanium oxide and magnesium oxide; the second hydrogenation active component is selected from one or more of nickel, molybdenum, tungsten and cobalt. In the method of the present invention, a non-precious metal catalyst is used as a hydrofining catalyst, which avoids the need to set up a gas stripping tower between the hydrotreatment reaction zone and the hydrofining reaction zone, thereby simplifying the process and making the operation easier.
[0051] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.
[0052] The properties of the raw materials used in the examples and comparative examples of the present invention are shown in Table 1.
[0053] Table 1
[0054] Raw material 1 Raw material 2 <![CDATA[Density at 20 °C, kg / m 3 > 839.9 841.6 Pour point, ℃ -15 -12 Sulfur content, % 0.438 0.115 Nitrogen content, mg / kg 142 253 Aromatic content, % 20.9 15.3 Distillation range (D86), ℃ Initial distillation point 157 210 10% 234 241 30% 259 264 50% 263 278 70% 274 294 90% 288 319 Do some work 308 346
[0055] The catalysts used in the examples and comparative examples of the present invention are prepared by the following method.
[0056] Preparation Example 1
[0057] Hydrogenation treatment catalyst A was prepared by the following method: 2000 g of aluminum hydroxide powder (dry rubber powder produced by the catalyst factory of Changling Branch, 72 wt% on a dry basis) was weighed and extruded into cylindrical strips with an circumscribed circle diameter of 1.3 mm using an extruder. The wet strips were dried at 120°C for 4 hours and calcined at 600°C for 3 hours to obtain carrier Sl.
[0058] Weigh 200 g of carrier S1, and soak the carrier in 176 ml of an aqueous solution containing 4.2 g of ammonium fluoride (analytical grade, a product of Beijing Chemical Plant) for 2 hours, dry at 120° C. for 3 hours, and roast at 420° C. for 3 hours to obtain a fluorine-containing aluminum oxide carrier. The above carrier was soaked in 170 ml of an aqueous solution containing 14.7 g of ammonium paramolybdate (chemically pure, a product of Beijing Chemical Plant) for 3 hours, dried at 120° C. for 8 hours, and then soaked in 162 ml of an aqueous solution containing 23.8 g of nickel nitrate (analytical grade, a product of Beijing Chemical Plant), 107.4 g of ammonium metatungstate (industrial grade, a product of Sichuan Zigong Cemented Carbide Plant) and 12.8 g of phosphoric acid for 3 hours. The wet strip was dried at 120° C. for 4 hours and roasted at 450° C. for 4 hours to obtain catalyst A, whose composition was determined by X-ray fluorescence.
[0059] Based on the dry weight of the hydroprocessing catalyst A, the mass fraction of nickel is 2.7%, the mass fraction of tungsten is 27.7%, the mass fraction of molybdenum is 3.3%, and the rest is the fluorine-containing alumina carrier, and the mass fraction of fluorine is 0.6% based on the dry weight of the catalyst A. The acidity of the catalyst or the carrier is characterized by pyridine adsorption-infrared spectroscopy, and the ratio of pyridine infrared B acid to L acid measured by the alumina carrier at 200°C is 0.165.
[0060] Preparation Example 2
[0061] Hydrogenation treatment catalyst B was prepared by the following method: 2000 g of aluminum hydroxide powder (dry rubber powder produced by the catalyst factory of Changling Branch, 72 wt% on a dry basis) was weighed and extruded into cylindrical strips with an circumscribed circle diameter of 1.3 mm using an extruder. The wet strips were dried at 120°C for 4 hours and calcined at 600°C for 3 hours to obtain carrier Sl.
[0062] Weigh 200 g of carrier S1, and impregnate the carrier with an aqueous solution containing 29.0 g of ammonium fluoride (analytical grade, product of Beijing Chemical Plant) for 2 hours, dry at 120°C for 3 hours, and roast at 420°C for 3 hours to obtain a fluorine-containing aluminum oxide carrier. The above carrier is impregnated with 170 ml of an aqueous solution containing 16.3 g of ammonium paramolybdate (chemically pure, product of Beijing Chemical Plant) for 3 hours, dried at 120°C for 8 hours, and then impregnated with 162 ml of an aqueous solution containing 30.2 g of nickel nitrate (analytical grade, product of Beijing Chemical Plant), 131.5 g of ammonium metatungstate (industrial grade, product of Sichuan Zigong Cemented Carbide Plant) and 18.5 g of phosphoric acid for 3 hours. The wet strip is dried at 120°C for 4 hours and roasted at 450°C for 4 hours to obtain catalyst B, whose composition is determined by X-ray fluorescence method.
[0063] Based on the dry weight of the hydroprocessing catalyst B, the mass fraction of nickel is 2.9%, the mass fraction of tungsten is 28.9%, the mass fraction of molybdenum is 3.1%, and the rest is the fluorine-containing alumina carrier, and the mass fraction of fluorine is 3.5% based on the dry weight of the catalyst B. The acidity of the catalyst or the carrier is characterized by pyridine adsorption-infrared spectroscopy, and the ratio of pyridine infrared B acid to L acid measured by the alumina carrier at 200°C is 0.614.
[0064] Preparation Example 3
[0065] Hydroprocessing catalyst C was prepared by the following method: 2000 g of aluminum hydroxide powder (dry rubber powder produced by the catalyst factory of Changling Branch, 72 wt% on a dry basis) was weighed and extruded into cylindrical strips with an circumscribed circle diameter of 1.3 mm using an extruder. The wet strips were dried at 120°C for 4 hours and calcined at 600°C for 3 hours to obtain carrier Sl.
[0066] Weigh 200 g of carrier S1, and soak the carrier in 175 ml of an aqueous solution containing 52.8 g of ammonium fluoride (analytical pure, a product of Beijing Chemical Plant) for 2 hours, dry at 120° C. for 3 hours, and roast at 420° C. for 3 hours to obtain a fluorine-containing aluminum oxide carrier. The above carrier was soaked in 170 ml of an aqueous solution containing 17.6 g of ammonium paramolybdate (chemically pure, a product of Beijing Chemical Plant) for 3 hours, dried at 120° C. for 8 hours, and then soaked in 162 ml of an aqueous solution containing 28.6 g of nickel nitrate (analytical pure, a product of Beijing Chemical Plant), 129.5 g of ammonium metatungstate (industrial grade, a product of Sichuan Zigong Cemented Carbide Plant) and 12.8 g of phosphoric acid for 3 hours. The wet strip was dried at 120° C. for 4 hours and roasted at 450° C. for 4 hours to obtain catalyst C, whose composition was determined by X-ray fluorescence.
[0067] Based on the dry weight of the hydroprocessing catalyst C, the mass fraction of nickel is 2.7%, the mass fraction of tungsten is 27.5%, the mass fraction of molybdenum is 3.2%, and the rest is the fluorine-containing alumina carrier, and the mass fraction of fluorine is 6.2% based on the dry weight of the catalyst C. The acidity of the catalyst or the carrier is characterized by pyridine adsorption-infrared spectroscopy, and the ratio of pyridine infrared B acid to L acid measured by the alumina carrier at 200°C is 1.39.
[0068] Preparation Example 4
[0069] Hydrogenation treatment catalyst D was prepared by the following method: 2000 g of aluminum hydroxide powder (dry rubber powder produced by the catalyst factory of Changling Branch, 72 wt% on a dry basis) was weighed and extruded into cylindrical strips with an circumscribed circle diameter of 1.3 mm using an extruder. The wet strips were dried at 120°C for 4 hours and calcined at 600°C for 3 hours to obtain carrier Sl.
[0070] Weigh 200 g of carrier S1, and soak the carrier in 176 ml of an aqueous solution containing 4.7 g of ammonium fluoride (analytical grade, a product of Beijing Chemical Plant) for 2 hours, dry at 120° C. for 3 hours, and roast at 420° C. for 3 hours to obtain a fluorine-containing aluminum oxide carrier. The above carrier was soaked in 170 ml of an aqueous solution containing 17.5 g of ammonium paramolybdate (chemically pure, a product of Beijing Chemical Plant) for 3 hours, dried at 120° C. for 8 hours, and then soaked in 162 ml of an aqueous solution containing 34.9 g of nickel nitrate (analytical grade, a product of Beijing Chemical Plant), 125.1 g of ammonium metatungstate (industrial grade, a product of Sichuan Zigong Cemented Carbide Plant) and 12.8 g of phosphoric acid for 3 hours. The wet strip was dried at 120° C. for 4 hours and roasted at 450° C. for 4 hours to obtain catalyst D, whose composition was determined by X-ray fluorescence.
[0071] Based on the dry weight of the hydroprocessing catalyst D, the mass fraction of nickel is 3.6%, the mass fraction of tungsten is 29.6%, the mass fraction of molybdenum is 3.6%, and the rest is the fluorine-containing alumina carrier, and the mass fraction of fluorine is 0.6% based on the dry weight of the catalyst D. The acidity of the catalyst or the carrier is characterized by pyridine adsorption-infrared spectroscopy, and the ratio of pyridine infrared B acid to L acid measured by the alumina carrier at 200°C is 0.162.
[0072] Preparation Example 5
[0073] Hydroprocessing catalyst E was prepared by the following method: 2000 g of aluminum hydroxide powder (dry rubber powder produced by the catalyst factory of Changling Branch, 72 wt% on a dry basis) was weighed and extruded into cylindrical strips with an circumscribed circle diameter of 1.3 mm using an extruder. The wet strips were dried at 120°C for 4 hours and calcined at 600°C for 3 hours to obtain carrier Sl.
[0074] Weigh 200 g of carrier S1, impregnate the carrier with 170 ml of an aqueous solution containing 46.3 g of ammonium paramolybdate (chemically pure, a product of Beijing Chemical Plant) for 3 hours, dry at 120°C for 8 hours, and then impregnate with 162 ml of an aqueous solution containing 40.8 g of nickel nitrate (analytical pure, a product of Beijing Chemical Plant), 110.5 g of ammonium metatungstate (industrial grade, a product of Sichuan Zigong Cemented Carbide Plant), and 14.2 g of phosphoric acid for 3 hours. Dry the wet strip at 120°C for 4 hours and calcine at 450°C for 4 hours to obtain catalyst E, whose composition is determined by X-ray fluorescence.
[0075] Based on the dry weight of the hydroprocessing catalyst E, the mass fraction of nickel is 4.1%, the mass fraction of tungsten is 25.1%, the mass fraction of molybdenum is 9.2%, and the rest is a fluorine-free alumina carrier. The acidity of the catalyst or the carrier is characterized by pyridine adsorption-infrared spectroscopy, and the ratio of pyridine infrared B acid to L acid measured by the alumina carrier at 200°C is 0.06.
[0076] Preparation Example 6
[0077] Hydrogenation treatment catalyst F was prepared by the following method: 2000 g of aluminum hydroxide powder (dry rubber powder produced by the catalyst factory of Changling Branch, 72 wt% on a dry basis) was weighed and extruded into cylindrical strips with an circumscribed circle diameter of 1.3 mm using an extruder. The wet strips were dried at 120°C for 4 hours and calcined at 600°C for 3 hours to obtain carrier Sl.
[0078] Weigh 200 g of carrier S1, and impregnate the carrier with an aqueous solution containing 62.4 g of ammonium fluoride (analytical grade, product of Beijing Chemical Plant) for 2 hours, dry at 120° C. for 3 hours, and roast at 420° C. for 3 hours to obtain a fluorine-containing aluminum oxide carrier. The above carrier is impregnated with 174 ml of an aqueous solution containing 18.9 g of ammonium paramolybdate (chemically pure, product of Beijing Chemical Plant) for 3 hours, dried at 120° C. for 8 hours, and then impregnated with 192 ml of an aqueous solution containing 30.7 g of nickel nitrate (analytical grade, product of Beijing Chemical Plant), 137.8 g of ammonium metatungstate (industrial grade, product of Sichuan Zigong Cemented Carbide Plant), and 16.8 g of phosphoric acid for 3 hours. The wet strip is dried at 120° C. for 4 hours and roasted at 450° C. for 4 hours to obtain catalyst F, whose composition is determined by X-ray fluorescence method.
[0079] Based on the dry weight of the hydroprocessing catalyst F, the mass fraction of nickel is 2.7%, the mass fraction of tungsten is 27.7%, the mass fraction of molybdenum is 3.3%, and the rest is the fluorine-containing alumina carrier, and the mass fraction of fluorine is 6.9% based on the dry weight of the catalyst F. The acidity of the catalyst or the carrier is characterized by pyridine adsorption-infrared spectroscopy, and the ratio of pyridine infrared B acid to L acid measured by the alumina carrier at 200°C is 1.720.
[0080] Preparation Example 7
[0081] The hydroprocessing catalyst G was prepared by the following method: 2000 g of aluminum hydroxide powder (dry rubber powder produced by the catalyst factory of Changling Branch, 72 wt% on a dry basis) was weighed and extruded into cylindrical strips with an circumscribed circle diameter of 1.3 mm using an extruder. The wet strips were dried at 120°C for 4 hours and calcined at 600°C for 3 hours to obtain the carrier Sl.
[0082] Weigh 200 g of carrier S1, impregnate the carrier with 170 ml of an aqueous solution containing 14.5 g of ammonium paramolybdate (chemically pure, a product of Beijing Chemical Plant) for 3 hours, dry at 120°C for 8 hours, and then impregnate with 165 ml of an aqueous solution containing 23.8 g of nickel nitrate (analytical pure, a product of Beijing Chemical Plant), 105.3 g of ammonium metatungstate (industrial grade, a product of Sichuan Zigong Cemented Carbide Plant), and 12.8 g of phosphoric acid for 3 hours. The wet strip is dried at 120°C for 4 hours and calcined at 450°C for 4 hours to obtain catalyst G, whose composition is determined by X-ray fluorescence.
[0083] Based on the dry weight of the hydroprocessing catalyst G, the mass fraction of nickel is 2.7%, the mass fraction of tungsten is 27.7%, the mass fraction of molybdenum is 3.3%, and the rest is alumina support. The acidity of the catalyst or support is characterized by pyridine adsorption-infrared spectroscopy, and the ratio of pyridine infrared B acid to L acid measured by the alumina support at 200°C is 0.07.
[0084] Preparation Example 8
[0085] Hydrorefining catalyst a was prepared by the following method: 2000 g of aluminum hydroxide powder (dry rubber powder produced by the catalyst plant of Sinopec Changling Branch, 70 wt% on dry basis) and 1400 g of silica sol (product of Qingdao Ocean Chemical Plant, with a silicon dioxide content of 25 wt%) were weighed and extruded into clover-shaped strips with a circumscribed circle diameter of 1.4 mm using an extruder. The wet strips were dried at 120° C. for 5 hours and then calcined at 550° C. for 6 hours to obtain carrier S2, in which the silicon dioxide content was 20.0 wt%. 100 g of carrier S2 was weighed and impregnated for 2 hours with 97 ml of an aqueous solution containing 5.8 g of ammonium metamolybdate, 30.5 g of nickel nitrate, 77.2 g of ammonium metatungstate and 12.5 g of ethylenediaminetetraacetic acid, and dried at 170° C. for 4 hours to obtain catalyst d. The composition of catalyst d after calcination was determined by X-ray fluorescence.
[0086] Based on the total amount of the hydrorefining catalyst a, calculated as oxides, the mass fraction of nickel is 5.5%, the mass fraction of tungsten is 32.0%, the mass fraction of molybdenum is 2.1%, and the rest is a silicon oxide-alumina carrier.
[0087] Example 1
[0088] like Figure 1 As shown, light white oil is prepared by the following method:
[0089] S1, in the presence of hydrogen, contacting the raw material 1 with a hydroprocessing catalyst A for hydroprocessing to obtain a hydroprocessing product;
[0090] S2. In the presence of hydrogen, contacting the hydrotreated product with a hydrorefining catalyst a for hydrorefining treatment to obtain a hydrorefined oil;
[0091] S3, fractionating the hydrorefined oil to obtain light white oil.
[0092] The operating conditions of each step are shown in Table 2, and the properties of the obtained products are shown in Table 3.
[0093] Table 2
[0094] Process conditions Hydroprocessing Hydrotreating Hydrogen partial pressure / MPa 15.0 15.0 Reaction temperature / ℃ 310 280 <![CDATA[Space velocity per hour -1 > 1.0 1.0 Hydrogen to oil ratio / (v / v) 600:1 600:1
[0095] Table 3
[0096]
[0097] Example 2
[0098] Light white oil was prepared by the same method as in Example 1, except that the conditions of the hydrotreating and hydrofining treatments were different from those in Example 1, as shown in Table 4. The properties of the obtained product are shown in Table 5.
[0099] Table 4
[0100] Process conditions Hydroprocessing Hydrotreating Hydrogen partial pressure / MPa 12.0 12.0 Reaction temperature / ℃ 340 300 <![CDATA[Space velocity per hour -1 > 1.0 1.0 Hydrogen to oil ratio / (v / v) 600:1 600:1
[0101] Table 5
[0102]
[0103] Example 3
[0104] Light white oil was prepared by the same method as in Example 1, except that hydrotreating catalyst B was used instead of hydrotreating catalyst A in step S1. The properties of the obtained product are shown in Table 6.
[0105] Table 6
[0106]
[0107]
[0108] Example 4
[0109] Industrial white oil and light white oil were prepared by the same method as in Example 1, except that raw material 2 was used instead of raw material 1 in step S1. The properties of the obtained products are shown in Table 7.
[0110] Table 7
[0111]
[0112] Example 5
[0113] Light white oil was prepared by the same method as in Example 1, except that hydrotreating catalyst C was used instead of hydrotreating catalyst A in step S1. The properties of the obtained product are shown in Table 8.
[0114] Table 8
[0115]
[0116] Example 6
[0117] Light white oil was prepared by the same method as in Example 1, except that hydrotreating catalyst D was used instead of hydrotreating catalyst A in step S1. The properties of the obtained product are shown in Table 9.
[0118] Table 9
[0119]
[0120] Comparative Example 1
[0121] Light white oil was prepared by the same method as in Example 1, except that hydrotreating catalyst E was used instead of hydrotreating catalyst A in step S1. The properties of the obtained product are shown in Table 10.
[0122] Table 10
[0123]
[0124] Comparative Example 2
[0125] Light white oil was prepared by the same method as in Example 1, except that hydrotreating catalyst G was used instead of hydrotreating catalyst A in step S1. The properties of the obtained product are shown in Table 11.
[0126] Table 11
[0127]
[0128] Comparative Example 3
[0129] Light white oil was prepared by the same method as in Example 1, except that hydrotreating catalyst F was used instead of hydrotreating catalyst A in step S1. The properties of the obtained product are shown in Table 10.
[0130] Table 10
[0131]
[0132] The method of the invention has small investment, simple process, easy operation, high yield of white oil, low aromatic content of the prepared product, and can meet the requirement of "light white oil II" for aromatic content in the light white oil standard.
[0133] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0134] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0135] In addition, any combination of the various embodiments of the present invention may be performed, and as long as it does not violate the concept of the present invention, it should also be regarded as the content disclosed by the present invention. In addition, any combination of the various embodiments of the present disclosure may be performed, and as long as it does not violate the concept of the present disclosure, it should also be regarded as the content disclosed by the present disclosure.
Claims
1. A method for producing light white oil and / or industrial white oil, the method include: S1. In the presence of hydrogen, the crude oil is contacted with a hydroprocessing catalyst for hydroprocessing to obtain a hydroprocessing product; The feedstock oil contains straight-run kerosene fraction and / or straight-run diesel fraction; the conditions of the hydrotreatment include: hydrogen partial pressure of 12-15 MPa, temperature of 280-310°C, volume space velocity of 0.5-1h -1 , the volume ratio of hydrogen to oil is (300-600):1; S2. In the presence of hydrogen, the hydrotreated product is contacted with a hydrorefining catalyst for hydrorefining treatment to obtain a hydrorefined oil; the conditions of the hydrorefining treatment include: a hydrogen partial pressure of 12-15 MPa, a temperature of 260-280° C., and a volume space velocity of 0.5-1 h -1 , the volume ratio of hydrogen to oil is (300-600):1; S3, separating the hydrorefined oil to obtain the light white oil and / or industrial white oil; The hydroprocessing catalyst is a non-precious metal catalyst; the hydroprocessing catalyst contains an alumina carrier and a first hydrogenation active component, the alumina carrier contains fluorine, and the ratio of B acid to L acid of pyridine infrared measured at 200°C of the alumina carrier is 0.16-1.35; the first hydrogenation active component is a VIB group metal and / or a VIII group metal; based on the dry weight of the hydroprocessing catalyst, the fluorine content is 0.5-6% by weight.
2. The method according to claim 1, in, The first hydrogenation active component is selected from one or more of Co, Ni, Mo and W; Based on the dry weight of the hydroprocessing catalyst, the content of the first hydrogenation active component is 1-34% by weight in terms of oxide.
3. The method according to claim 1, in, The distillation range of the raw oil is 120-400°C, and the pour point is -50°C to -6°C.
4. The method according to claim 1, in, The method comprises: contacting the feedstock oil with the hydroprocessing catalyst in a hydroprocessing reaction zone to perform the hydroprocessing; then contacting the obtained hydroprocessing product with the hydroprocessing catalyst in a hydrofining reaction zone to perform the hydrofining treatment; The feedstock oil contains a straight-run kerosene fraction and a straight-run diesel fraction, and the straight-run kerosene fraction and the straight-run diesel fraction are alternately fed into the hydroprocessing reaction zone in a switching feed manner.
5. The method according to claim 1, in, In step S3, the separation includes: distilling the hydrorefined oil to obtain light white oil and / or industrial white oil.
6. The method according to claim 1, in, The hydrotreating catalyst is a non-precious metal catalyst; The hydrotreating catalyst contains a second hydrogenation active component and an inert carrier; The inert carrier includes one or more of silicon oxide, aluminum oxide, titanium oxide and magnesium oxide; the second hydrogenation active component is selected from one or more of nickel, molybdenum, tungsten and cobalt.