Preparation method and application of spherical pure phase tungsten diboride
By heating and pressurizing tungsten powder and boron powder in an oxygen-free atmosphere, combined with self-mixing and spheroidizing treatments, tungsten diboride powder with high sphericity, fluidity and purity was prepared, solving the two problems in the existing technology. The difficult problem of tungsten boride powder preparation enables the production of high-quality materials suitable for additive manufacturing.
Patent Information
- Application Number
- CN202211584909.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-09
AI Technical Summary
It is difficult to effectively prepare tungsten diboride powder with high sphericity, fluidity and purity with existing technology, which limits its application in additive manufacturing.
Spherical pure-phase tungsten diboride is prepared by mixing tungsten powder and boron powder, performing heating and pressure treatment in an oxygen-free atmosphere, and then performing self-mixing treatment and spheroidization treatment. The method includes predispersing tungsten powder and boron powder, controlling the molar ratio and particle size, avoiding oxidation and side reactions, improving reaction efficiency and purity, and improving fluidity and sphericity rate through self-mixing and spheroidization.
The obtained tungsten diboride has high sphericity, fluidity and bulk density, which meets the needs of additive manufacturing. It has a single phase and no impurities, making it suitable for industrial production.
Smart Images

Figure CN116081633B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of powder metallurgy, and in particular relates to a preparation method and application of spherical pure-phase tungsten diboride. Background Art
[0002] Tungsten-boron compounds have a wide range of applications due to their high melting point, high hardness, high electrical conductivity and excellent wear resistance. At the same time, due to the high atomic number of tungsten, it has a good shielding effect on gamma rays, and the boron element has a high neutron absorption cross-section and a wide absorption energy range, making tungsten-boron compounds a new type of nuclear shielding material that can shield both gamma rays and neutrons. At present, tungsten-boron nuclear shielding materials are mostly prepared by additive manufacturing. Compared with traditional technologies, additive manufacturing technology has high material utilization and fewer processing steps, which is conducive to the design of complex workpieces. However, additive manufacturing technology has high requirements for raw material powders. Powders with high sphericity, good fluidity and high purity are more conducive to the smooth progress of additive manufacturing. Therefore, how to obtain tungsten diboride that can be used for additive manufacturing needs further research. Summary of the invention
[0003] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to propose a method for preparing spherical pure phase tungsten diboride and its application. The method is not only simple in process and suitable for industrial production, but also the prepared tungsten diboride has a single phase without other impurities, and has a high sphericity, good fluidity, and high bulk density, which can meet the use requirements of additive manufacturing.
[0004] In one aspect of the present invention, the present invention provides a method for preparing spherical pure phase tungsten diboride. According to an embodiment of the present invention, the method comprises:
[0005] (1) mixing tungsten powder and boron powder to obtain mixed powder;
[0006] (2) heating and pressurizing the mixed powder in an oxygen-free atmosphere to obtain pure phase tungsten diboride;
[0007] (3) performing a self-mixing treatment on the pure phase tungsten diboride to obtain a tungsten diboride self-mixed powder;
[0008] (4) Spheroidizing the tungsten diboride self-mixed powder to obtain spherical pure phase tungsten diboride.
[0009] The method for preparing spherical pure phase tungsten diboride in the above embodiment of the present invention has at least the following beneficial effects: 1) the tungsten powder and the boron powder are pre-dispersed first to fully mix the two, which is more conducive to the subsequent full reaction of the tungsten powder and the boron powder, thereby not only improving the reaction efficiency, but also reducing the occurrence of side reactions and improving the purity of the tungsten diboride product; 2) the reaction of the tungsten powder and the boron powder is carried out under the conditions of oxygen-free atmosphere, heating and pressurization. The oxygen-free atmosphere can prevent the tungsten powder and the boron powder from being oxidized to produce impurities. The pressure can reduce the loss of the boron powder due to sublimation at high temperature, which can be more accurate. Determine the demand for boron powder and reduce the waste of raw materials. On the other hand, the mass ratio of tungsten powder and boron powder can be combined to avoid the generation of other intermediate compounds (such as WB, WB4, etc.) except tungsten diboride to a great extent, which is more conducive to ensuring the uniformity of the tungsten diboride phase; 3) By self-mixing the pure phase tungsten diboride, the edges and corners of the tungsten diboride particles can be reduced, the fluidity of the powder can be improved, which is conducive to the smooth powder feeding process during the subsequent spheroidization treatment, thereby not only improving the spheroidization efficiency, but also improving the spheroidization treatment effect, so that the final product has a higher sphericity and better fluidity.
[0010] In addition, the method for preparing spherical pure phase tungsten diboride according to the above embodiment of the present invention may also have the following additional technical features:
[0011] In some embodiments of the present invention, step (1) satisfies at least one of the following conditions: the molar ratio of the tungsten powder to the boron powder is 1:(2.05-2.15), the tungsten powder is obtained by the following method: the tungsten powder is passed through an 80-mesh sieve to obtain an oversize material, the boron powder has a particle size of 2-5 μm, and the mixing is performed by ball milling.
[0012] In some embodiments of the present invention, the ball milling treatment has a rotation speed of 100-200 r / min, a time of 10-60 min, and a ball-to-material ratio of (0.2-2):1; and / or, tungsten powder with an average particle size of 15-30 μm is sieved through an 80-mesh sieve to obtain a sieve-surface material.
[0013] In some embodiments of the present invention, in step (2), the temperature of the heating and pressurizing treatment is 1100-1600° C., the pressure is 0.05-0.15 MPa, and the time is 1-6 h; and / or the oxygen-free atmosphere is an inert gas atmosphere and / or a nitrogen atmosphere.
[0014] In some embodiments of the present invention, in step (3), the frequency of the self-mixing treatment is 20 to 60 Hz and the time is 15 to 60 min; and / or, after the self-mixing treatment, the self-mixing product is further screened.
[0015] In some embodiments of the present invention, in step (3), the self-mixed product is sieved through a 140-mesh sieve, and the sieve-less product is taken as the tungsten diboride self-mixed powder.
[0016] In some embodiments of the present invention, in step (4), the spheroidization treatment adopts a plasma spheroidization process; and / or the spheroidal rate of the spherical pure phase tungsten diboride is not less than 80%, the fluidity is not higher than 6.5s / 50g, and the bulk density is not less than 9.5g / cm 3 .
[0017] In some embodiments of the present invention, the plasma spheroidization process meets the following conditions: the powder carrier gas flow rate is 6 to 14 L / min, the plasma gas flow rate is 2 to 6 L / min, the feed speed is 0.5 to 6 r / min, and the current is 100 to 130 A.
[0018] In another aspect of the present invention, the present invention proposes spherical pure phase tungsten diboride prepared by the above method for preparing spherical pure phase tungsten diboride. Compared with the prior art, the tungsten diboride has a single phase, no other impurities, high sphericity, good fluidity, and high bulk density, which can meet the use requirements of additive manufacturing.
[0019] In another aspect of the present invention, the present invention proposes the above method for preparing spherical pure phase tungsten diboride and / or the use of the above spherical pure phase tungsten diboride in preparing tungsten-boron shielding materials by additive manufacturing. This use has all the technical features and effects of the above method for preparing spherical pure phase tungsten diboride and the above spherical pure phase tungsten diboride, which will not be repeated here. In general, the use of this method and spherical pure phase tungsten diboride is more conducive to the preparation of tungsten-boron shielding materials by additive manufacturing.
[0020] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0022] Figure 1 is a flow chart of a method for preparing pure phase spherical tungsten diboride according to one embodiment of the present invention;
[0023] Figure 2 It is the standard X-ray diffraction pattern of tungsten diboride;
[0024] Figure 3 is the X-ray diffraction pattern of the final product prepared according to Example 1 of the present invention;
[0025] Figure 4 is a scanning electron microscope (SEM) image of the final product obtained according to Example 1 of the present invention, wherein Figure 4 A and Figure 4 Middle and b are SEM images at different magnifications;
[0026] Figure 5 is the X-ray diffraction pattern of the final product prepared according to Comparative Example 1 of the present invention;
[0027] Figure 6 is a scanning electron microscope (SEM) image of the final product prepared according to Comparative Example 1 of the present invention;
[0028] Figure 7 is the X-ray diffraction pattern of the final product prepared according to Comparative Example 2 of the present invention;
[0029] Figure 8 is a scanning electron microscope (SEM) image of the final product prepared according to Comparative Example 2 of the present invention;
[0030] Fig. 9 is a scanning electron microscope (SEM) image of the final product prepared according to Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0031] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in the art or the product specifications are used.
[0032] In one aspect of the present invention, a method for preparing spherical pure phase tungsten diboride is proposed. According to an embodiment of the present invention, the method comprises: (1) mixing tungsten powder and boron powder to obtain a mixed powder; (2) heating and pressurizing the mixed powder in an oxygen-free atmosphere to obtain a pure phase tungsten diboride; (3) performing a self-mixing treatment on the pure phase tungsten diboride to obtain a tungsten diboride self-mixed powder; (4) performing a spheroidizing treatment on the tungsten diboride self-mixed powder to obtain a spherical pure phase tungsten diboride. Compared with the prior art, the method for preparing spherical pure phase tungsten diboride of the present invention has at least the following beneficial effects: 1) the tungsten powder and the boron powder are pre-dispersed first to make the two fully mixed, which is more conducive to the subsequent full reaction of the tungsten powder and the boron powder, thereby not only improving the reaction efficiency, but also reducing the occurrence of side reactions and improving the purity of the tungsten diboride product; 2) the reaction of the tungsten powder and the boron powder is carried out under the conditions of oxygen-free atmosphere, heating and pressurization. The oxygen-free atmosphere can prevent the tungsten powder and the boron powder from being oxidized to produce impurities. The pressure can reduce the loss of the boron powder caused by sublimation at high temperature, which can be more accurate. On the one hand, the demand for boron powder can be determined to reduce the waste of raw materials. On the other hand, the mass ratio of tungsten powder and boron powder can be combined to avoid the generation of other intermediate compounds (such as WB, WB4, etc.) except tungsten diboride to a great extent, which is more conducive to ensuring the uniformity of the tungsten diboride phase; 3) By self-mixing the pure phase tungsten diboride, the edges and corners of the tungsten diboride particles can be reduced, the fluidity of the powder can be improved, which is conducive to the smooth powder feeding process during the subsequent spheroidization treatment, thereby not only improving the spheroidization efficiency, but also improving the spheroidization treatment effect, so that the final product has a higher sphericity and better fluidity.
[0033] Reference below Figure 1 The method for preparing spherical pure phase tungsten diboride according to the above embodiment of the present invention is described in detail.
[0034] S100: Mix tungsten powder and boron powder to obtain mixed powder
[0035] According to the embodiment of the present invention, mixing tungsten powder and boron powder can promote the subsequent reaction of tungsten powder and boron powder to be fully carried out, improve reaction efficiency, reduce the occurrence of side reactions, and improve the purity of the obtained tungsten diboride product.
[0036] According to an embodiment of the present invention, the molar ratio of tungsten powder to boron powder can be 1:(2.05-2.15), for example, 1:2.08, 1:2.1, 1:2.12 or 1:2.14. The inventors found that boron powder is prone to partial loss due to sublimation under high temperature conditions. If the molar ratio of tungsten powder to boron powder is too small, in the subsequent heating and pressurizing process, it is easy to cause the molar ratio of boron powder and tungsten powder participating in the reaction to be less than 2:1, which is easy to increase side reactions, and the product may be doped with impurities such as tungsten monoboride, resulting in a decrease in the purity of tungsten diboride; and if the molar ratio of tungsten powder to boron powder is too large, it is also easy to increase side reactions, and the product may be doped with impurities such as tungsten tetraboride, resulting in a decrease in the purity of tungsten diboride. In the present invention, by controlling the molar ratio of tungsten powder to boron powder to be within the above range, and combining the subsequent heating and pressurizing reaction, it is not only more conducive to obtaining pure phase tungsten diboride, but also can reduce the waste of raw materials.
[0037] According to an embodiment of the present invention, tungsten powder can be obtained in the following manner: tungsten powder is passed through an 80-mesh sieve to obtain an oversize material, for example, tungsten powder with an average particle size of 15 to 30 μm is passed through an 80-mesh sieve to obtain an oversize material, and the oversize material is mixed with boron powder. The particle size of the boron powder can be 2 to 5 μm, for example, 2.5 μm, 3 μm, 3.5 μm, 4 μm or 4.5 μm, etc. The inventors found that the tungsten diboride prepared by the reaction of tungsten powder with larger particle size and boron powder also has a larger particle size, and the fluidity of tungsten diboride with larger particle size is relatively good, which is more conducive to the smooth progress of the powder feeding process during the subsequent spheroidization treatment of tungsten diboride, and the obtained tungsten diboride powder with larger size and higher sphericity rate can better meet the use requirements of additive manufacturing; if the particle size of the tungsten powder is too small, the fluidity of the tungsten diboride obtained by the reaction is also relatively poor, which is not conducive to the powder feeding operation during the subsequent spheroidization treatment. By passing the tungsten powder through an 80-mesh sieve, a tungsten powder with a more concentrated particle size distribution can be obtained, and the average particle size range of the obtained tungsten powder is also relatively large; in addition, boron powder with a particle size of 2 to 5 μm can be combined with tungsten powder of the above-mentioned particle size, filled into the gaps between tungsten powder particles, and fully contacted with the tungsten powder, thereby improving the reaction efficiency and conversion rate under subsequent heating and pressurization conditions. In summary, in the present invention, by comprehensively controlling the particle sizes of tungsten powder and boron powder to be within the above range, it is not only beneficial to the sufficient contact reaction between the two, but also beneficial to improve the particle size and fluidity of the subsequently obtained pure phase tungsten diboride, ensure the powder feeding efficiency and spheroidization effect of the subsequent spheroidization process, and obtain spherical pure phase tungsten diboride with high sphericity, good fluidity and high loose density.
[0038] According to an embodiment of the present invention, when tungsten powder and boron powder are mixed, ball milling can be used. The present invention does not particularly limit the ball milling device, and those skilled in the art can flexibly select it according to actual conditions, for example, a horizontal planetary ball milling device can be used.
[0039] According to a specific embodiment of the present invention, during the ball milling process, the rotation speed can be 100 to 200 r / min, for example, 120 r / min, 150 r / min, 160 r / min or 180 r / min, etc. The inventors found that if the ball milling speed is too low, it is difficult to achieve uniform mixing of tungsten powder and boron powder; if the ball milling speed is too high, the powder is subjected to a strong impact and is more likely to be broken, resulting in a significant decrease in the particle size of the powder, which is not conducive to improving the particle size and fluidity of the tungsten diboride powder obtained later. In addition, at high speeds, the grinding balls are also prone to being in a centrifugal state, and it is also difficult to achieve uniform mixing of tungsten powder and boron powder. In the present invention, by controlling the rotation speed of the ball milling process within the above range, not only can the tungsten powder and boron powder be fully mixed and evenly dispersed, but also the reduction in particle size caused by the grinding of the powder can be avoided as much as possible, thereby ensuring the fluidity of the powder in the subsequent process.
[0040] According to a specific embodiment of the present invention, during the ball milling process, the ball milling time can be 10 to 60 minutes, for example, 15 minutes, 20 minutes, 30 minutes, 40 minutes or 50 minutes. The inventors found that if the ball milling time is too short, it is difficult to achieve sufficient mixing and uniform dispersion of tungsten powder and boron powder; and if the ball milling time is too long, the friction and collision time between the grinding media (such as stainless steel balls) or between the grinding media and the inner surface of the equipment is long, which will increase the risk of introducing impurities. At the same time, long-term grinding and impact are also likely to cause a significant reduction in the particle size of the powder, reducing the fluidity of the pure phase tungsten diboride obtained subsequently. In the present invention, by controlling the ball milling time to the above range, it is more conducive to obtaining pure phase tungsten diboride with good fluidity.
[0041] According to a specific embodiment of the present invention, during the ball milling process, the ball-to-material ratio can be (0.2-2):1, for example, it can be 0.5:1, 1:1, 1.5:1 or 1.8:1. The inventors found that if the ball-to-material ratio is too large, the friction and collision frequency between the grinding media and between the grinding media and the inner wall of the equipment will also be large, which will not only increase the degree of powder crushing, reduce the particle size, reduce the fluidity of the powder, but also increase the risk of introducing impurities; and if the ball-to-material ratio is too small, the number of collisions of a small number of grinding media on the powder is also small, and it is difficult to ensure the dispersion effect of tungsten powder and boron powder. In the present invention, by controlling the ball-to-material ratio within the above range, it is more conducive to obtaining pure phase and good fluidity tungsten diboride. Preferably, during the ball milling process, the ball-to-material ratio can be (0.5-1.5):1, which can further facilitate the acquisition of pure phase and good fluidity tungsten diboride, and improve the powder feeding efficiency and spheroidization effect during subsequent spheroidization.
[0042] S200: Heat and pressurize the mixed powder in an oxygen-free atmosphere to obtain pure phase tungsten diboride
[0043] According to an embodiment of the present invention, during the heating and pressurizing process, controlling the oxygen-free atmosphere can prevent tungsten powder and boron powder from being oxidized and introducing impurities, and pressurizing can reduce the loss of boron powder due to sublimation at high temperature. On the one hand, it can reduce the waste of boron powder, and on the other hand, it can combine the mass ratio of tungsten powder and boron powder and the stoichiometric ratio of tungsten diboride to avoid the generation of other intermediate compounds (such as WB, WB4, etc.) except tungsten diboride to a great extent, which is more conducive to ensuring the uniform phase of tungsten diboride.
[0044] According to an embodiment of the present invention, the oxygen-free atmosphere may be an inert gas atmosphere and / or a nitrogen atmosphere. Among them, the use of inert gas and / or nitrogen to form an oxygen-free condition can not only prevent tungsten powder and boron powder from being oxidized and then introducing impurities, but also provide the required pressure conditions for heating and pressurizing treatment. For example, according to some specific embodiments of the present invention, during the heating and pressurizing treatment, before or after the mixed powder is added to the reaction equipment (such as a reactor), the air in the equipment can be first extracted, and inert gas and / or nitrogen can be introduced. After repeated multiple times, the air in the reaction equipment is fully replaced to form an oxygen-free environment; thereafter, the amount of inert gas and / or nitrogen introduced is adjusted to reach the target pressure value in the reaction equipment. It can be understood that the pressure regulation process can be carried out simultaneously with the heating operation, or the pressure in the reaction equipment can be adjusted to the target value before the heating operation is carried out. After reaching the expected reaction temperature, the temperature is kept to allow the tungsten powder and the boron powder to fully react to obtain pure phase tungsten diboride. It should be noted that the reaction equipment used for the heating and pressurizing treatment in the present invention is not particularly limited, and those skilled in the art can flexibly select it according to actual needs, for example, it can be a vacuum high-temperature chamber furnace bell, etc.
[0045] According to an embodiment of the present invention, the temperature of the heating and pressurizing treatment can be 1100-1600°C, for example, 1200°C, 1300°C, 1400°C or 1500°C, etc.; the pressure can be 0.05-0.15MPa, for example, 0.08MPa, 0.1MPa, 0.12MPa or 0.14MPa, etc.; the insulation time can be 1-6h, for example, 2h, 3h, 4h or 5h, etc. The inventors found that if the heating temperature is too low, the side reactions are relatively active in the process of generating tungsten diboride, the conversion rate of tungsten monoboride increases significantly, and the purity of the tungsten diboride product is reduced. If the heating temperature is too high, the sublimation of boron powder will be aggravated. When the boron powder content is low, the impurity content in the final product will also increase, and it is difficult to obtain a single phase of tungsten diboride; if the pressurization pressure is too low, the sublimation and volatilization of boron powder cannot be effectively suppressed. If the pressure is too high, the material is easily hardened and not easy to break; if the insulation time is too short, it is difficult to ensure the full reaction between tungsten powder and boron powder, which easily leads to a low yield of tungsten diboride and low purity. If the insulation time is too long, on the one hand, the probability of generating impurities will increase, and on the other hand, it will also cause energy waste and increase production costs. In the present invention, by controlling the temperature, pressure and insulation time of the heating and pressurization treatment within the above range, the purity of the tungsten diboride product can be further improved under the premise of ensuring the full reaction of tungsten powder and boron powder, and pure phase tungsten diboride can be obtained.
[0046] S300: self-mixing the pure phase tungsten diboride to obtain tungsten diboride self-mixed powder
[0047] According to an embodiment of the present invention, by performing self-mixing treatment on pure phase tungsten diboride, the edges and corners of the tungsten diboride particles can be reduced, the fluidity of the powder can be improved, and the smooth powder feeding operation during the subsequent spheroidization treatment can be facilitated, thereby not only improving the spheroidization efficiency, but also improving the spheroidization treatment effect, so that the final product has a higher sphericity and better fluidity.
[0048] According to an embodiment of the present invention, the frequency of the self-mixing treatment can be 20 to 60 Hz, for example, 25 Hz, 30 Hz, 40 Hz, 50 Hz or 55 Hz, etc.; the self-mixing time can be 15 to 60 min, for example, 20 min, 25 min, 30 min, 40 min, 50 min or 55 min, etc. It should be noted that the self-mixing treatment does not add grinding media. The inventors found that by self-mixing pure phase tungsten diboride, the friction between the tungsten diboride powders can weaken the edges and corners of the particle surface, improve the fluidity of the tungsten diboride powder, and help improve the powder feeding efficiency during the subsequent spheroidization treatment, thereby optimizing the spheroidization treatment effect and improving the sphericity of the product. However, if the rotation speed of the self-mixing treatment is too low or the self-mixing time is too short, it is difficult for tungsten diboride to achieve the effect of self-grinding. If the rotation speed of the self-mixing treatment is too high or the self-mixing time is too long, the interaction between the tungsten diboride powder itself or the powder and the inner wall of the equipment is too strong, which can easily lead to further crushing of the tungsten diboride powder, reduce the fluidity of the powder, and be unfavorable for the subsequent powder feeding operation of the spheroidization treatment. In the present invention, the rotation speed of the self-mixing treatment is indirectly controlled by controlling the frequency of the self-mixing treatment. By controlling the frequency and time of the self-mixing treatment to be within the above range, it is possible to avoid the introduction of other impurities and significantly reduce the surface edges and corners of the pure phase tungsten diboride particles on the basis of avoiding a significant decrease in the particle size, making the surface smoother and having better fluidity.
[0049] According to an embodiment of the present invention, the self-mixing process may further include: screening the self-mixed product. Through the screening process, the particle size distribution of tungsten diboride can be made more concentrated, which is more conducive to controlling the thickness of the printing layer and the dimensional accuracy of the workpiece during the additive manufacturing process. According to a specific embodiment of the present invention, the tungsten diboride self-mixed powder can be passed through a 140-mesh sieve, and the sieve underfill can be retained, thereby ensuring the fluidity of tungsten diboride and facilitating the powder feeding operation during the spheroidization process, and also facilitating the acquisition of spherical pure phase tungsten diboride particles with more uniform size, thereby being more conducive to improving the printing accuracy of the additive manufacturing process using tungsten powder as raw material.
[0050] S400: Spheroidize the tungsten diboride self-mixed powder to obtain spherical pure phase tungsten diboride
[0051] According to an embodiment of the present invention, by performing a spheroidization treatment, the sphericity and fluidity of the spherical pure phase tungsten diboride finally obtained can be further guaranteed. It should be noted that the specific method of the spheroidization treatment is not particularly limited in the present invention, and those skilled in the art can flexibly select it according to the actual situation. For example, the spheroidization treatment can adopt a plasma spheroidization treatment process. Among them, the plasma spheroidization treatment can use hot ions to provide a high temperature environment, and the tungsten diboride is sent into the high temperature plasma through a carrier gas. After the tungsten diboride particles quickly absorb heat, the surface (or the whole) melts, and condenses under the action of surface tension to form spherical droplets, and then the spherical droplets enter the cooling chamber, solidify after rapid cooling, and fix the sphere to obtain spherical pure phase tungsten diboride.
[0052] According to an embodiment of the present invention, in the plasma spheroidization treatment: the powder carrier gas flow rate can be 6-14L / min, for example, 7L / min, 8L / min, 10L / min, 12L / min or 13L / min, etc.; the plasma gas flow rate can be 2-6L / min, for example, 3L / min, 4L / min or 5L / min, etc.; the feed speed can be 0.5-6r / min, for example, 1r / min, 2r / min, 3r / min, 4r / min or 5r / min, etc.; the current can be 100-130A, for example, 105A, 110A, 115A, 120A or 125A, etc. The inventors found that in the plasma spheroidization treatment process, the powder carrier gas flow rate, the plasma gas flow rate, the feed speed and the current The size of the powder carrier gas will affect the efficiency and effect of plasma spheroidization. For example, if the powder feeding carrier gas flow rate is too large, the powder feeding efficiency is high, and the number of powders passing through the high-temperature area of the plasma moment per unit time is large, which may easily lead to a single particle absorbing less heat, and then it will be difficult for more powders to be effectively spheroidized, affecting the spheroidization effect of tungsten diboride particles. If the powder feeding carrier gas flow rate is too small, the powder feeding efficiency is low, and the powder absorbs too much heat, which may cause the powder to sublimate, affecting the product yield, and also increasing energy consumption; at the same time, if the plasma gas flow rate is too large or the current is too large, it may also cause low product yield and increased energy consumption due to sublimation. If the plasma gas flow rate is too small or the current is too small, it may also cause the powder to be difficult to be effectively spheroidized, resulting in reduced spheroidization efficiency and effect; in addition, the feed speed will also affect the powder feeding rate, thereby affecting the efficiency or effect of the spheroidization effect. In the present invention, by controlling the plasma spheroidization process within the above parameter range, it is more conducive to improving the spheroidization effect of tungsten diboride, while ensuring the spheroidization efficiency and yield, and obtaining spherical pure phase tungsten diboride with high sphericity, good fluidity and high bulk density. Specifically, the obtained spherical pure phase tungsten diboride can achieve the following effects: sphericity is not less than 80%, fluidity is not higher than 6.5s / 50g, and bulk density is not less than 9.5g / cm 3 , which can meet the use requirements of additive manufacturing.
[0053] In another aspect of the present invention, the present invention proposes spherical pure phase tungsten diboride prepared by the above method for preparing spherical pure phase tungsten diboride. Compared with the prior art, the tungsten diboride has a single phase, no other impurities, high sphericity, good fluidity, and high bulk density, which can meet the use requirements of additive manufacturing. For example, the spherical pure phase tungsten diboride can simultaneously meet the following requirements: sphericity not less than 80%, fluidity not less than 6.5s / 50g, and bulk density not less than 9.5g / cm 3 It should be noted that the characteristics and effects described for the above method for preparing spherical pure phase tungsten diboride are also applicable to the spherical pure phase tungsten diboride, and will not be described in detail here.
[0054] In another aspect of the present invention, the present invention proposes the above-mentioned method for preparing spherical pure phase tungsten diboride and / or the use of the above-mentioned spherical pure phase tungsten diboride in preparing tungsten-boron shielding materials by additive manufacturing. This use has all the technical features and effects of the above-mentioned method for preparing spherical pure phase tungsten diboride, which will not be repeated here. In general, the use of this method and spherical pure phase tungsten diboride is more conducive to the preparation of tungsten-boron shielding materials by additive manufacturing.
[0055] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.
[0056] Example 1
[0057] (1) Take tungsten powder with an average particle size of 20 μm and pass it through an 80-mesh sieve, retain the tungsten powder on the sieve, and mix it with boron powder with an average particle size of 3 μm in a molar ratio of 1:2.1. The mixing process adopts a horizontal planetary ball milling equipment, uses spherical ball milling media, a ball-to-material ratio of 0.5:1, a mixing speed of 150 r / min, and a mixing time of 30 min to obtain a mixed powder;
[0058] (2) adding the mixed powder into a vacuum high-temperature box furnace, heating and pressurizing the mixture in an argon atmosphere, pressurizing the mixture to 0.1 MPa with argon, heating the mixture to 1400° C. and maintaining the temperature for 2 h to obtain tungsten diboride powder;
[0059] (3) adding tungsten diboride powder to a mixer and mixing it by itself without adding a ball milling medium; the operating frequency of the mixer is 50 Hz, and the mixing time is 30 min. After the mixing is completed, the mixing product is passed through a 140-mesh sieve, and the sieve-under is taken to obtain tungsten diboride self-mixed powder;
[0060] (4) The above-mentioned tungsten diboride self-mixed powder is added to a plasma spheroidization device for spheroidization treatment, wherein the powder feeding carrier gas flow rate is 10 L / min, the plasma gas flow rate is 4 L / min, the feed speed is 1.5 r / min, and the current is 120 A to obtain the final tungsten diboride.
[0061] Embodiments 2 to 4
[0062] The difference from Example 1 is shown in Table 1
[0063] Comparative Examples 1 to 3
[0064] The difference from Example 1 is shown in Table 1
[0065] Performance testing and evaluation:
[0066] Under the same conditions, the tungsten diboride prepared in Examples 1 to 4 and Comparative Examples 1 to 3 was characterized by the following test methods, including: phase composition, sphericity, fluidity and bulk density. The characterization results are shown in Tables 1 and Figures 2 to 9 shown.
[0067] Test method:
[0068] Phase composition: carried out by X-ray diffraction;
[0069] Sphericity: According to the Sphericity Determination Method of Nickel-Based Superalloy Powders (YS / T 1491-2021), scanning electron microscopy method;
[0070] Fluidity: According to GB / T 1482-2010, the standard funnel method for the determination of the fluidity of metal powders (Hall flow meter);
[0071] Bulk density: According to GB / T 1479.2-2011 Determination of bulk density of metal powders Part 2: Scott volumetric meter method.
[0072] Table 1 Process parameters and test results of Examples 1 to 4 and Comparative Examples 1 to 3
[0073]
[0074]
[0075] Results and Discussion:
[0076] Combining the test results of Examples 1 to 4 and Comparative Examples 1 to 3, it can be seen that the tungsten diboride obtained in Examples 1 to 4 has a single phase and no impurity phase; the sphericity is high, all greater than 80%; the fluidity is good, all better than 6.5s / 50g; the bulk density is large, all not less than 9.5g / cm 3 .
[0077] Among them, combined Figures 2-3 understand, Figure 2 is the standard XRD spectrum of tungsten diboride; Figure 3 The XRD spectrum of the final product tungsten diboride of Example 1 is Figure 2 The peak positions of the standard spectrum shown in FIG. 1 are consistent, and there are no other impurity peaks, indicating that the final product of Example 1 is pure phase tungsten diboride, and there is no other impurity phase; the XRD spectra of tungsten diboride of the final products of Examples 2 to 4 are consistent with those of Example 1 and the standard spectrum. Figure 1 The results are consistent, which also shows that pure phase tungsten diboride is obtained. Figure 4 a and b are SEM images of the final product of Example 1 at different magnifications. Figure 4 It can be clearly seen that the sphericity of the tungsten diboride product obtained in Example 1 is relatively high. Combined with the industry standard "YS / T 1491-2021 Nickel-based high-temperature alloy powder sphericity determination method scanning electron microscopy method", it is calculated that the sphericity of the pure phase tungsten diboride in Example 1 is 90%. The SEM images of the final products of Examples 2 to 4 are basically consistent with Example 1, indicating that the sphericity of the tungsten diboride products obtained in Examples 2 to 4 is also relatively high. Based on the calculation of the sphericity of the products based on the SEM images, it can be seen that the sphericity of the tungsten diboride products obtained in Examples 2 to 4 is greater than 80%.
[0078] in addition, Figure 5 The XRD spectrum of the final product obtained in Comparative Example 1 (the XRD spectrum corresponding to Figure 2 The same peak position of the WB2 standard spectrum and the WB standard spectrum shown in the figure) Figure 6 The SEM image of the final product obtained in Comparative Example 1 is shown in FIG. Figure 5 According to the analysis, there is tungsten boride (WB) in the final product of Comparative Example 1. This is because the molar ratio of boron powder to tungsten powder added in Comparative Example 1 is low, and the reaction of generating WB is more active, resulting in a decrease in the purity of the WB2 product. Figure 6 Analysis shows that the sphericity of the final product obtained in Comparative Example 1 is also significantly reduced. Figure 7 The XRD spectrum of the final product obtained in Comparative Example 2 (the XRD spectrum corresponding to Figure 2 The same peak position of the WB2 standard spectrum and the WB standard spectrum shown in the figure) Figure 8 The SEM image of the final product obtained in Comparative Example 2 is shown in FIG. Figure 7 According to the analysis, in the final product of Comparative Example 2, WB becomes the main phase and WB2 becomes the secondary phase. This is because the reaction temperature is low and the reaction process is dominated by the reaction of generating WB, which leads to a significant decrease in the purity of the product. At the same time, due to the change in the phase composition and the unchanged plasma spheroidization process, the sphericity of the product is also significantly reduced (such as Figure 8 shown). Fig. 9This is a SEM image of the final product obtained in Comparative Example 3. Compared with Example 1, the sphericity, fluidity and loose density of the product in Comparative Example 3 are all reduced, which may be caused by changing the plasma spheroidization process parameters.
[0079] In summary, the method for preparing spherical pure phase tungsten diboride according to the above embodiment of the present invention can obtain pure phase tungsten diboride, and the tungsten diboride has high sphericity, high fluidity, and high bulk density, which can meet the needs of additive manufacturing.
[0080] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0081] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing spherical pure phase tungsten diboride, It is characterized in that include: (1) Mixing tungsten powder and boron powder to obtain mixed powder; (2) heating and pressurizing the mixed powder in an oxygen-free atmosphere to obtain pure phase tungsten diboride; (3) performing a self-mixing treatment on the pure phase tungsten diboride to obtain a tungsten diboride self-mixing powder; (4) spheroidizing the tungsten diboride self-mixed powder to obtain spherical pure phase tungsten diboride; Step (1) satisfies at least one of the following conditions: The molar ratio of the tungsten powder to the boron powder is 1:(2.05-2.15); The tungsten powder is obtained by the following method: passing the tungsten powder through an 80-mesh sieve to obtain the sieve-surface material; The boron powder particle size is 2-5 μm; In step (2), the temperature of the heating and pressurizing treatment is 1100-1600°C, the pressure is 0.05-0.15 MPa, and the time is 1-6 hours; In step (4), the spheroidization treatment adopts a plasma spheroidization process; The plasma spheroidization treatment process meets the following conditions: the powder carrier gas flow rate is 6-14 L / min, the plasma gas flow rate is 2-6 L / min, the feed speed is 0.5-6 r / min, and the current is 100-130 A.
2. The method according to claim 1, It is characterized in that The mixing is performed by ball milling.
3. The method according to claim 2, It is characterized in that The ball milling process has a rotation speed of 100-200 r / min, a time of 10-60 min, and a ball-to-material ratio of (0.2-2):1; and / or, Tungsten powder with an average particle size of 15-30 μm is sieved through an 80-mesh sieve to obtain the sieve-surface material.
4. The method according to claim 1, It is characterized in that In step (2), the oxygen-free atmosphere is an inert gas atmosphere and / or a nitrogen atmosphere.
5. The method according to claim 1, It is characterized in that In step (3), the frequency of the self-mixing treatment is 20-60 Hz and the time is 15-60 min; and / or, After the self-mixing process, the method further comprises: screening the self-mixing product.
6. The method according to claim 1 or 5, It is characterized in that In step (3), the self-mixed product is sieved through a 140-mesh sieve, and the sieve-less product is taken as the tungsten diboride self-mixed powder.
7. The method according to claim 1, It is characterized in that In step (4), the spherical pure phase tungsten diboride has a sphericity of not less than 80%, a fluidity of not more than 6.5s / 50g, and a bulk density of not less than 9.5g / cm 3 .
8. Spherical pure phase tungsten diboride is prepared by the method according to any one of claims 1 to 7.
9. Use of the spherical pure phase tungsten diboride prepared by the method of any one of claims 1 to 7 and / or the spherical pure phase tungsten diboride according to claim 8 in preparing tungsten-boron-based nuclear shielding materials by additive manufacturing.
Citation Information
Patent Citations
High-fluidity pure-phase tungsten diboride and preparation method thereof
CN116199229A