A high-strength austenitic stainless steel powder and preparation method thereof
By adjusting the material composition and sintering process of austenitic stainless steel and adding Ni and Mo elements, the high strength and hardness of austenitic stainless steel in metal powder injection molding is achieved, and the uneven magnetic properties and performance of traditional austenitic stainless steel are solved. The problem of simplifying the process flow and improving corrosion resistance and non-magnetic properties.
Patent Information
- Application Number
- CN202310153679.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Traditional austenitic stainless steel produces magnetic properties after a large amount of deformation and processing, which cannot meet the requirements of high mechanical properties. In addition, uneven nitrogen infiltration during metal powder injection molding leads to uneven performance, complex process and high cost.
By adjusting the material composition and adding Ni and Mo elements, it is fully austenitized in a non-nitrogen environment, avoiding nitriding treatment, and combining appropriate sintering and degreasing treatment, ensuring the corrosion resistance and non-magnetic properties of the material, while improving the Strength and hardness.
It realizes the strength and hardness of austenitic stainless steel while maintaining corrosion resistance and non-magnetic properties, simplifying the process flow, avoiding heat treatment steps, and improving the performance and production efficiency of the material.
Smart Images

Figure CN116083819B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of materials for powder injection molding, and in particular relates to a high-strength austenitic stainless steel powder and a preparation method thereof. Background Art
[0002] Powder injection molding is a new component forming processing technology that introduces plastic injection molding technology into the field of powder metallurgy. It is to mix powder (metal powder, ceramic powder) with an organic binder into a uniform feed, granulate it and then inject it into the molded blank, and then degrease it and sinter it to densify it into the desired finished product. Since this process is a net size forming process, it has the advantages of high material utilization, can be directly formed into complex shapes, high batch production efficiency, and high dimensional accuracy. Since the 1990s, it has continued to develop rapidly, and more and more various materials have been successfully commercially applied using injection molding technology.
[0003] Austenitic stainless steel is widely used in decoration, kitchenware, electronic products and other fields due to its excellent corrosion resistance and mechanical properties. The more representative ones are 304 and 316L. However, austenitic stainless steel cannot significantly improve its strength and hardness through heat treatment. In the traditional casting field, its strength and hardness can be improved through work hardening. However, after a large amount of deformation processing, the austenitic structure produces deformation-induced martensite and magnetism, which cannot meet the requirements for magnetic properties. Therefore, its application is limited in fields with higher requirements for mechanical properties. Therefore, how to make austenitic stainless steel retain good corrosion resistance and non-magnetic properties while having better strength and hardness has become a new research direction.
[0004] Patent announcement number CN105839022B discloses a high-hardness non-magnetic nickel-free stainless steel and a manufacturing method thereof, wherein the chemical composition by weight percentage is: C: 0.15-0.20%, Si: 0.2-0.8%, Mn: 17.0-19.0%, Cr: 13.5-14.5%, N: 0.25-0.30%, Cu: 0.5-0.8%, B: 0.0015-0.0040%, the hardness is HV 425-497, the yield strength is 1100-1350MPa, and the magnetic phase content is 0%.
[0005] However, its composition contains 0.25-0.30% nitrogen. For metal powder injection molding, the addition of nitrogen needs to be infiltrated through a nitrogen atmosphere during the sintering process. However, the material is densified during sintering, and the nitriding will be very uneven, so it is easy for the nitrogen content and performance to be uneven in different parts.
[0006] Patent announcement number CN112981231B discloses a high manganese nitrogen austenitic stainless steel powder, which relates to the technical field of alloy material powder preparation, and is characterized in that: the high manganese nitrogen austenitic stainless steel powder also includes the following components calculated by weight percentage: Mn: 9.00%-10.00%, S: ≤0.003%, P: ≤0.05%, Si: 0.30%-0.80%, Cr: 13.00%-15.00%, Ni: 1.00%-2.00%, B: 0.00 2%-0.004%, Cu: 0.20%-1.0%, its yield strength after injection molding and sintering is ≥300MPa, tensile strength ≥650MPa, elongation ≥40%, hardness ≥85HRB, but for metal powder injection molding, the cooling rate is slow during cooling, and the nitrogen dissolved in the matrix will precipitate and form compounds with chromium, resulting in chromium-poor material matrix, which has a great impact on corrosion resistance. Subsequent solution treatment is required to re-dissolve nitrogen in the matrix, and the process flow is complicated and the cost is high. Summary of the invention
[0007] In view of the above problems, the present invention provides a high-strength austenitic stainless steel powder and a preparation method thereof, which improves the strength and hardness of the material while ensuring its corrosion resistance and non-magnetic properties.
[0008] The present invention adopts the following technical scheme: a high-strength austenitic stainless steel powder, characterized in that it includes the following components: calculated by weight percentage, carbon content ≤0.10wt.%, oxygen content ≤0.20wt.%, nitrogen content ≤0.20wt.%, Cr: 15%-17%, Mn: 6%-8%, Mo: 3.899%-5%, Ni: 8.311%-11%, Si: ≤1.0%, P: ≤0.03%, S≤0.03%, and Fe as the balance.
[0009] Preferably, the tap density of the powder is 4.5 g / cm3-5.0 g / cm 3 , bulk density is 3.9g / cm 3 -4.4g / cm 3 .
[0010] Preferably, the stainless steel powder has a D10 of 3-5 μm, a D50 of 11-14 μm, and a D90 of 25-28 μm.
[0011] The present invention also discloses a method for preparing a powder injection molding product, which is characterized in that the temperature of an internal mixer is set to 170-190°C, the stirring speed is 15-20 r / min, the above-mentioned stainless steel powder, polymer adhesive and coupling agent are added, and stirring is carried out for 0.5-2h, then the temperature is lowered to 160-180°C, a lubricating dispersant is added, and stirring is continued for 0.5-2h to obtain a mixed agglomerated feed and start granulation, the granulation extrusion speed is 10-20 r / min, the pelletizing speed is 10-20 r / min, the injection feed is obtained, and the finished product is made through degreasing and sintering.
[0012] Preferably, the debinding and sintering process is as follows: the debinding blank is placed in a sintering furnace, the temperature is raised to 400-600°C for 1-6 hours, and the temperature is kept at 400-600°C for 2-8 hours, and the remaining polymer adhesive is removed by heating decomposition. After thermal debinding, all the adhesives are removed completely, and then the temperature is continued to be raised to the sintering temperature. After sintering, heat preservation and cooling, a sintered and dense finished product is obtained.
[0013] The metal powder sintered product prepared by the method is characterized by tensile strength ≥500Mpa, yield strength ≥200Mpa, elongation ≥40%, hardness ≥150HV1, and magnetic permeability ≤1.01.
[0014] The present invention uses the traditional high-manganese austenitic stainless steel and adjusts the material composition so that it does not need nitriding in the sintering process. It has good corrosion resistance and non-magnetic properties, and has better strength and hardness performance, and does not need to be subjected to heat treatment after sintering. By adding a certain amount of Ni element to the material, it can be fully austenitized in a non-nitrogen environment to achieve the purpose of non-magnetism. The addition of Mo element can improve the corrosion resistance on the one hand, and on the other hand, it can weaken the tendency to form continuous network carbides and refine the grains, so that the material does not need nitriding or heat treatment during sintering, and can also achieve the purpose of non-magnetism and high hardness. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 These are the microscopic metallographic images of Example 1 at 200X and 500X.
[0016] Figure 2 These are the microscopic metallographic images of Example 2 at 200X and 500X.
[0017] Figure 3 These are the microscopic metallographic images of Example 3 at 200X and 500X. DETAILED DESCRIPTION
[0018] The present invention is further described below in conjunction with specific embodiments.
[0019] Comparative Example 1
[0020] The composition of the metal powder is as follows:
[0021]
[0022] Feeding: Stainless steel metal powder and binder are added to the internal mixing tank, the temperature of the internal mixing tank is raised to 185°C, and the speed is 15r / min for internal mixing for 0.5h; the temperature of the internal mixing tank is lowered to 165°C, stearic acid is added, stirring is continued for 1h, and then extrusion is performed for granulation.
[0023] Injection molding: conventional injection process.
[0024] Thermal degreasing in nitric acid atmosphere: degreasing temperature 110℃, degreasing time: 12h.
[0025] Sintering: thermal debinding process, heating to 600℃ for 4h, and keeping at 600℃ for 3h. Sintering process: 1380℃ / 3h argon protective atmosphere sintering. The performance results are as follows:
[0026]
[0027] Implementation case 1:
[0028] The composition of the metal powder, calculated by weight percentage, is as follows:
[0029]
[0030] Feeding: Stainless steel metal powder and binder are added to the internal mixing tank, the temperature of the internal mixing tank is raised to 185°C, and the speed is 15r / min for internal mixing for 0.5h; the temperature of the internal mixing tank is lowered to 165°C, stearic acid is added, stirring is continued for 1h, and then extrusion is performed for granulation.
[0031] Injection molding: conventional injection process.
[0032] Thermal degreasing in nitric acid atmosphere: degreasing temperature 110℃, degreasing time: 12h.
[0033] Sintering: hot debinding process, heating to 600℃ for 4h, keeping at 600℃ for 3h. Sintering process: 1290℃ / 3h argon protective atmosphere sintering. The performance results are as follows:
[0034]
[0035]
[0036] Implementation case 2:
[0037] The composition of the metal powder is as follows:
[0038]
[0039] Feeding: Add stainless steel metal powder and binder into the internal mixing tank, heat the internal mixing tank to 185℃, and mix at a speed of 15r / min for 0.5h; lower the temperature of the internal mixing tank to 165℃, add stearic acid, continue stirring for 1h, and then extrude and granulate. Injection molding: conventional injection process.
[0040] Thermal degreasing in nitric acid atmosphere: degreasing temperature 110℃, degreasing time: 12h.
[0041] Sintering: hot debinding process, heating to 600℃ for 4h, keeping at 600℃ for 3h. Sintering process: 1290℃ / 3h argon protective atmosphere sintering. The performance results are as follows:
[0042]
[0043] Implementation case three:
[0044] The composition of the metal powder is as follows:
[0045]
[0046] Feeding: Add stainless steel metal powder and binder into the internal mixing tank, heat the internal mixing tank to 185℃, and mix at a speed of 15r / min for 0.5h; lower the temperature of the internal mixing tank to 165℃, add stearic acid, continue stirring for 1h, and then extrude and granulate. Injection molding: conventional injection process.
[0047] Thermal degreasing in nitric acid atmosphere: degreasing temperature 110℃, degreasing time: 12h.
[0048] Sintering: hot debinding process, heating to 600℃ for 4h, keeping at 600℃ for 3h. Sintering process: 1290℃ / 3h argon protective atmosphere sintering. The performance results are as follows:
[0049]
[0050]
[0051] The table below shows the room temperature mechanical properties of high-strength austenitic stainless steel. Its strength is significantly better than traditional austenitic stainless steels such as 304 and 316.
[0052]
[0053] Mechanical properties of injection molded 316 stainless steel: tensile strength ≥440Mpa, yield strength ≥110Mpa, elongation ≥50%, hardness 120HV.
[0054] Traditional austenitic stainless steel has low hardness and strength under the premise of meeting the requirements of corrosion resistance and non-magnetism, which limits its application range. Traditional high manganese nitrogen austenitic stainless steel is not suitable for the field of metal powder injection molding because the nitrogen element in the material can only be infiltrated during sintering, and the nitriding effect of different parts is different due to different product structures, and the process control is relatively complicated. In addition, since nitrides will precipitate when the sintering process is cooled, it must be re-dissolved in the matrix through a heat treatment process to improve corrosion resistance and non-magnetism, and the entire process flow is relatively complicated.
[0055] The present invention adjusts the material composition on the basis of traditional high-manganese austenitic stainless steel, so that it does not need nitriding in the sintering process, has good corrosion resistance and non-magnetic properties, has better strength and hardness performance, and does not need heat treatment process after sintering.
[0056] By adding a certain amount of Ni element to the material, it can be fully austenitized in a non-nitrogen environment to achieve the purpose of non-magnetism. The addition of Mo element can improve the corrosion resistance on the one hand, and weaken the tendency to form continuous network carbides on the other hand, refine the grains, so that the material does not need nitriding or heat treatment during sintering, and can achieve the purpose of non-magnetism and high hardness.
[0057] It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.
Claims
1. A high-strength austenitic stainless steel powder, characterized in that The invention comprises the following components: calculated by weight percentage, carbon content ≤0.10wt.%, oxygen content ≤0.20wt.%, nitrogen content ≤0.20wt.%, Cr: 15%-17%, Mn: 6%-8%, Mo: 3.899%-5%, Ni: 8.311%-11%, Si: ≤1.0%, P: ≤0.03%, S≤0.03%, and Fe is the balance.
2. The high-strength austenitic stainless steel powder according to claim 1, characterized in that The tap density of the powder is 4.5 g / cm 3 -5.0g / cm 3 , bulk density is 3.9g / cm 3 -4.4g / cm 3 .
3. A high-strength austenitic stainless steel powder according to claim 1 or 2, characterized in that D10: 3-5μm, D50: 11-14μm, D90: 25-28μm.
4. A method for preparing a powder injection molding product, characterized in that The temperature of the internal mixer is set to 170-190° C., the stirring speed is 15-20 r / min, the stainless steel powder as described in any one of claims 1-3, the polymer binder and the coupling agent are added, and the stirring is carried out for 0.5-2 h, and then the temperature is reduced to 160-180° C., the lubricating dispersant is added, and the stirring is continued for 0.5-2 h to obtain the mixed agglomerated feed and start granulation, the granulation extrusion speed is 10-20 r / min, the pelletizing speed is 10-20 r / min, and the injection feed is obtained, which is degreased and sintered to form a finished product.
5. The method for preparing a powder injection molding product according to claim 4, characterized in that The debinding and sintering process is as follows: the debinding blank is placed in a sintering furnace, the temperature is raised to 400-600°C for 1-6 hours, and the temperature is kept at 400-600°C for 2-8 hours. The remaining polymer adhesive is removed by heating decomposition. After thermal debinding, all the adhesives are removed completely, and then the temperature is continued to be raised to the sintering temperature. After sintering, keeping the temperature and cooling, a sintered and dense finished product is obtained.
6. A metal powder sintered product obtained by the method of claim 4 or 5, characterized in that Tensile strength ≥500Mpa, yield strength ≥200Mpa, elongation ≥40%, hardness ≥150HV1, magnetic permeability ≤1.01.