A composite lithium adsorbent and preparation method thereof
The one-step synthesis method of alumina gel-loaded lithium manganese ion sieve is prepared, which solves the problems of complex process, high cost and low yield in the prior art, and achieves efficient and environmentally friendly lithium adsorption effect. Suitable for a variety of lithium processes.
Patent Information
- Application Number
- CN202310041127.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-01-13
AI Technical Summary
The existing lithium adsorbent preparation methods have problems such as complex process, high cost, low yield, low adsorption amount and poor permeability after forming, which is difficult to meet the needs of industrial applications.
The composite lithium adsorbent is prepared by a one-step synthesis method of aluminum oxide gel-loaded lithium manganese ion sieve. The aluminum source solution is hydrolyzed, added lithium source and manganese source, and the pore-forming agent is dried, molded and calcined, and finally activated in the acid solution to achieve the Complex lithium adsorbent with high porosity and high specific surface area.
Simplified the preparation process, reduced the loss of adsorption capacity, improved the adsorption rate and hydrophilicity, and was suitable for alkaline lithium-containing solutions, low-concentration lithium-containing solutions and salt lake brine lithium extraction processes. The material is wear-resistant and has an adsorption capacity after recycling. Maintaining 90% reduces costs.
Smart Images

Figure CN116099497B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal metallurgical separation and resource recycling, and in particular relates to a composite lithium adsorbent and a preparation method thereof. Background Art
[0002] Lithium and its compounds are strategic resources of great significance in the national economy and national defense construction, and are widely used in the battery, metallurgy and other industries. The world's proven onshore lithium resource reserves are about 14 million tons in terms of metallic lithium, of which 70% to 80% are in salt lake brine. At present, traditional lithium extraction technologies mainly include precipitation, salting out, solvent extraction, etc. The components of salt lake brine are complex, and traditional extraction methods have shortcomings such as complex process flow and high energy consumption; while ion exchange and adsorption method for lithium extraction has the advantages of good selective adsorption, simple process, and high recovery rate, and has developed into a very promising lithium extraction method.
[0003] Commonly used lithium adsorbents include ion exchange resins, ion imprinted materials, aluminum salt layered materials, ion sieves, etc. Ion sieve type adsorbents have the advantages of high adsorption capacity and good lithium-magnesium selectivity, and are lithium adsorption materials with good application prospects.
[0004] CN114289000A discloses a salt lake lithium extraction adsorbent and a preparation method thereof. The salt lake lithium extraction adsorbent contains the following raw materials in parts by weight: 40-60 parts of titanium source, 20-30 parts of lithium source, 5-10 parts of swelling organic polymer, 10-15 parts of strong acid solution with a mass fraction of 10-15%, 5-10 parts of solid carrier, 0.1-0.3 parts of dispersant, 0.2-0.5 parts of first porogen, 10-15 parts of sodium chloride solution, 5-10 parts of silicone oil. 0 parts, 1-2 parts of cross-linking agent, 5-8 parts of sodium chloride solution and 15-20 parts of sodium hydroxide solution with a mass fraction of 10-15%; the preparation method comprises: adding titanium ion sieve powder, cross-linking agent and kaolin powder to maleic anhydride grafted polyethylene wax to mix to obtain a modified solid carrier mixture, adding pore-forming agent, swelling organic polymer, dispersant and sodium chloride to mix, hot pressing into a film at 100-120°C and 120-160MPa to obtain an adsorbent. The preparation method uses the raw materials in combination to increase the adsorption amount, increase the permeability and adsorption rate, and shorten the adsorption time of the prepared adsorbent.
[0005] However, the above method has a long preparation time, low yield, low adsorption capacity, and high cost. In addition, since the direct application of the ion sieve powder in the industrial adsorption and desorption device will lead to problems such as poor permeability of the adsorption tower and large pressure drop, it needs to be molded.
[0006] Therefore, there is an urgent need to develop a method for preparing a lithium adsorbent with simple preparation process, low cost, environmental protection, high efficiency and shaped form. Summary of the invention
[0007] The object of the present invention is to provide a composite lithium adsorbent and a preparation method thereof. The preparation method synthesizes the composite lithium adsorbent by loading a lithium manganese ion sieve on alumina gel. The preparation method is simple in process and reduces the loss of adsorption capacity after the ion sieve is formed. The prepared composite lithium adsorbent can be used in alkaline lithium-containing solutions, low-concentration lithium-containing solutions and lithium-containing salt lake brine extraction processes.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a composite lithium adsorbent, the preparation method comprising the following steps:
[0010] (1) After the aluminum source solution is subjected to a first hydrolysis, a lithium source and a manganese source are added to perform a second hydrolysis to obtain an aluminum oxide composite gel;
[0011] (2) mixing the pore-forming agent and the alumina composite gel described in step (1), and then drying, molding and calcining in sequence to obtain a composite lithium adsorbent precursor;
[0012] (3) Activating the composite lithium adsorbent precursor described in step (2) to obtain a composite lithium adsorbent.
[0013] The preparation method of the present invention adopts alumina gel to mix lithium source, manganese source and pore-forming agent, and calcines a composite lithium adsorbent with high porosity, high specific surface area and doped with aluminum in one step, and simultaneously realizes ion sieve synthesis and molding. The alumina-loaded lithium manganese ion sieve is prepared by a one-step synthesis method, which shortens the synthesis process of the composite lithium adsorbent, reduces the loss of adsorption capacity after the ion sieve is molded, improves the hydrophilicity of the composite lithium adsorbent, and improves the adsorption rate.
[0014] As a preferred technical solution of the present invention, the aluminum source in the aluminum source solution of step (1) includes any one of aluminum chloride, aluminum isopropoxide, triethylaluminum, triisobutylaluminum, diisobutylaluminum hydride, monomethylaluminum hydride, dimethylaluminum hydride and triethylamine alane, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of aluminum chloride and aluminum isopropoxide, a combination of triethylaluminum and triisobutylaluminum, or a combination of diisobutylaluminum hydride and monomethylaluminum hydride, etc., preferably triethylaluminum or aluminum isopropoxide.
[0015] Preferably, the concentration of the aluminum source solution in step (1) is 1.5-3.5 mol / L, for example, it can be 1.5 mol / L, 1.7 mol / L, 2 mol / L, 2.4 mol / L, 2.8 mol / L, 3 mol / L or 3.5 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0016] Preferably, the temperature of the first hydrolysis in step (1) is 25-95°C, for example, 25°C, 35°C, 45°C, 55°C, 65°C, 75°C, 85°C or 95°C, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably 50-90°C.
[0017] Preferably, the first hydrolysis in step (1) is carried out under stirring conditions.
[0018] Preferably, the rotation speed of the first hydrolysis in step (1) is 100-500 rpm, for example, it can be 100 rpm, 200 rpm, 300 rpm, 400 rpm or 500 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] As a preferred technical solution of the present invention, in step (1), the acid solution is added after the first hydrolysis for 1-2 hours.
[0020] In the present invention, adding an acid solution after the first hydrolysis for 1-2 hours can promote the hydrolysis.
[0021] Preferably, the acid solution comprises nitric acid and / or hydrochloric acid.
[0022] Preferably, the concentration of the acid solution is 1-2 mol / L, for example, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L or 2 mol / L, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] As a preferred technical solution of the present invention, in step (1), the lithium source and the manganese source are added after the first hydrolysis for 2-4 hours.
[0024] Preferably, the lithium source in step (1) comprises any one of lithium carbonate, lithium nitrate, lithium acetate, lithium oxalate, lithium chloride, lithium hydroxide or lithium sulfate, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of lithium carbonate and lithium nitrate, a combination of lithium acetate and lithium oxalate, or a combination of lithium chloride and lithium hydroxide, etc., preferably lithium hydroxide or lithium carbonate.
[0025] Preferably, the manganese source in step (1) comprises any one of manganese carbonate, manganese dioxide, potassium permanganate, manganese carbonate or manganese nitrate, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of manganese carbonate and manganese dioxide, a combination of manganese dioxide and potassium permanganate, or a combination of manganese carbonate and manganese nitrate, etc., preferably manganese carbonate or manganese dioxide.
[0026] Preferably, the molar ratio of the lithium source to the manganese source in step (1) is (0.6-1):1, for example, it can be 0.6:1, 0.65:1, 0.7:1, 0.75:1, 0.8:1, 0.95:1 or 1:1, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] It is worth noting that the molar ratio of the aluminum source to the lithium source in the aluminum source solution of step (1) is (2.43-10.06):1. When the molar ratio of the aluminum source to the lithium source is controlled within a certain range, the number of lithium sites after activation is further controlled, which is beneficial to increase the adsorption amount and improve the stability of the material.
[0028] Preferably, the temperature of the second hydrolysis in step (1) is 70-95°C, for example, 70°C, 75°C, 80°C, 85°C, 90°C or 95°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the time for the second hydrolysis in step (1) is 15-24 h, for example, 15 h, 17 h, 20 h, 21 h, 22 h, 23 h or 24 h, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] As a preferred technical solution of the present invention, the pore-forming agent in step (2) includes any one of graphite, activated carbon, polyvinyl alcohol, polyvinyl chloride, calcium silicate or calcium carbonate, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of graphite and activated carbon, a combination of polyvinyl alcohol and polyvinyl chloride, or a combination of calcium silicate and calcium carbonate, etc., preferably graphite or calcium carbonate.
[0031] Preferably, the mass ratio of the pore-forming agent in step (2) to the alumina composite gel in step (1) is (0.1%-3%):1, for example, it can be 0.1%:1, 0.5%:1, 1%:1, 1.5%:1, 2%:1, 2.5%:1 or 3%:1, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the mixing time in step (2) is 20-60 min, for example, 20 min, 30 min, 40 min, 50 min or 60 min, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] As a preferred technical solution of the present invention, the drying temperature in step (2) is 50-100°C, for example, it can be 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably 60-70°C.
[0034] Preferably, the drying time in step (2) is 3-10 h, for example, 3 h, 4 h, 5 h, 6 h, 7 h, 9 h or 10 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] Preferably, the molding in step (2) is extrusion molding.
[0036] It is worth noting that the present invention adopts extrusion molding to achieve column adsorption of composite lithium adsorbent, and the composite lithium adsorbent has high wear resistance. After being recycled for 5 times, the adsorption capacity is still maintained at 90%, which reduces the adsorption cost.
[0037] Preferably, the heating rate of the calcination in step (2) is 4-8°C / min, for example, 4°C / min, 5°C / min, 6°C / min, 7°C / min or 8°C / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] Preferably, the calcination temperature in step (2) is 120-600°C, for example, it can be 120°C, 150°C, 200°C, 300°C, 400°C, 500°C or 600°C, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably 400-600°C.
[0039] Preferably, the holding time for calcination in step (2) is 4-6 h, for example, 4 h, 4.4 h, 4.8 h, 5 h, 5.4 h, 5.8 h or 6 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] In the present invention, the calcination is performed under air atmosphere.
[0041] As a preferred technical solution of the present invention, the activation treatment in step (3) is carried out in an acid solution.
[0042] Preferably, the acid solution comprises nitric acid and / or hydrochloric acid.
[0043] Preferably, the concentration of the acid solution is 0.1-0.5 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0045] (1) performing a first hydrolysis of a 1.5-3.5 mol / L aluminum source solution at 25-95° C. and a rotation speed of 100-500 rpm for 1-2 hours, adding an acid solution at a concentration of 1-2 mol / L, adding a lithium source and a manganese source after the first hydrolysis for 2-4 hours, and performing a second hydrolysis at 70-95° C. for 15-24 hours to obtain an alumina composite gel;
[0046] The molar ratio of the lithium source to the manganese source is (0.6-1):1;
[0047] (2) mixing the pore-forming agent and the alumina composite gel of step (1) for 20-60 minutes, drying at 50-100° C. for 3-10 hours, extruding and molding, and then heating to 120-600° C. at a heating rate of 4-8° C. / min, calcining and keeping the temperature for 4-6 hours to obtain a composite lithium adsorbent precursor;
[0048] The mass ratio of the pore-forming agent to the alumina composite gel in step (1) is (0.1%-3%): 1;
[0049] (3) Activating the composite lithium adsorbent precursor of step (2) in an acid solution with a concentration of 0.1-0.5 mol / L to obtain a composite lithium adsorbent.
[0050] In a second aspect, the present invention provides a composite lithium adsorbent prepared by the preparation method described in the first aspect.
[0051] In the present invention, the composite lithium adsorbent is a composite strip material of Al2O3 loaded with aluminum-doped manganese-based ion sieve.
[0052] As a preferred technical solution of the present invention, the porosity of the composite lithium adsorbent is 0.270-0.300m 3 / g, for example, it can be 0.270m 3 / g, 0.275m 3 / g, 0.280m 3 / g, 0.285m 3 / g, 0.290m 3 / g, 0.295m 3 / g or 0.300m 3 / g, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0053] Preferably, the specific surface area of the composite lithium adsorbent is 150-160m 2 / g, for example, it can be 150m 2 / g, 152m 2 / g, 154m 2 / g, 156m 2 / g, 158m 2 / g or 160m 2 / g, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] In the present invention, the composite lithium adsorbent is a strip-shaped mesoporous material.
[0055] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] (1) The preparation method of the present invention adopts a one-step synthesis method to prepare alumina-loaded lithium manganese ion sieve to realize ion sieve molding, shortens the synthesis process of the composite lithium adsorbent, reduces the loss of adsorption capacity after ion sieve molding, and improves the hydrophilicity of the composite lithium adsorbent; the preparation method does not generate harmful organic waste gas, generates less waste acid and waste alkali, and has no impact on the environment;
[0058] (2) The composite lithium adsorbent prepared by the present invention has high porosity and high specific surface area, and can be used in the lithium extraction process of alkaline lithium-containing solution, low-concentration lithium-containing solution and lithium-containing salt lake brine. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 A schematic flow chart of a method for preparing a composite lithium adsorbent provided by the present invention;
[0060] Figure 2 This is a BET characterization result diagram of the composite lithium adsorbent prepared in Example 1;
[0061] Figure 3 This is the pore size distribution diagram of the composite lithium adsorbent prepared in Example 1. DETAILED DESCRIPTION
[0062] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0063] The present invention provides a method for preparing a composite lithium adsorbent, the schematic diagram of which is as follows: Figure 1 As shown, the preparation method comprises the following steps:
[0064] (1) After the aluminum source solution is subjected to a first hydrolysis, a lithium source and a manganese source are added to perform a second hydrolysis to obtain an aluminum oxide composite gel;
[0065] (2) mixing the pore-forming agent and the alumina composite gel described in step (1), and then drying, extruding and calcining in sequence to obtain a composite lithium adsorbent precursor;
[0066] (3) Activating the composite lithium adsorbent precursor described in step (2) to obtain a composite lithium adsorbent.
[0067] Example 1
[0068] This embodiment provides a method for preparing a composite lithium adsorbent, the preparation method comprising the following steps:
[0069] (1) 100 mL of 1.5 mol / L aluminum isopropoxide aqueous solution was first hydrolyzed at 85° C. and 260 rpm for 1.5 h, then heated to 95° C., 30 mL of 1 mol / L nitric acid was added, 4.6 g of Li2CO3 and 17.9 g of MnCO3 were added after the first hydrolysis for 2 h, and the second hydrolysis was performed at 95° C. for 24 h to obtain an alumina composite gel;
[0070] (2) 0.5 g of graphite and the alumina composite gel described in step (1) were mixed in a blue sand mill at a speed of 3000 rpm for 30 min, then dried at 70° C. for 4 h, extruded by a screw extruder, and then heated to 600° C. at a heating rate of 5° C. / min for calcination and kept at this temperature for 4 h to obtain a composite lithium adsorbent precursor;
[0071] (3) Activating the composite lithium adsorbent precursor in step (2) in 0.2 mol / L hydrochloric acid to obtain a composite lithium adsorbent.
[0072] The composite lithium adsorbent prepared in this example was subjected to 5 adsorption-desorption experiments. After 5 cycles of use, it still had excellent adsorption performance, and the adsorption capacity only decreased from 25 mg / g to 21 mg / g.
[0073] Figure 2 This is a BET characterization result diagram of the composite lithium adsorbent prepared in this example. Figure 3 is the pore size distribution diagram of the composite lithium adsorbent prepared in this embodiment, Figure 2-3 It can be seen that the porosity of the composite lithium adsorbent is 0.286m 3 / g, specific surface area is 151m 2 / g.
[0074] Example 2
[0075] This embodiment provides a method for preparing a composite lithium adsorbent, the preparation method comprising the following steps:
[0076] (1) 200 mL of 1.5 mol / L aluminum isopropoxide aqueous solution was first hydrolyzed at 90° C. and 260 rpm for 1.5 h, then heated to 95° C., 30 mL of 1 mol / L nitric acid was added, 9.2 g of Li2CO3 and 35.8 g of MnCO3 were added after the first hydrolysis for 2 h, and the second hydrolysis was performed at 95° C. for 20 h to obtain an alumina composite gel;
[0077] (2) mixing 1 g of graphite and the alumina composite gel described in step (1) in a blue sand mill at a speed of 3000 rpm for 30 min, then drying at 70° C. for 4 h, extruding and molding using a screw extruder, and then heating to 600° C. at a heating rate of 5° C. / min, calcining and keeping the temperature for 4 h to obtain a composite lithium adsorbent precursor;
[0078] (3) Activating the composite lithium adsorbent precursor in step (2) in 0.3 mol / L hydrochloric acid to obtain a composite lithium adsorbent.
[0079] Example 3
[0080] This embodiment provides a method for preparing a composite lithium adsorbent, the preparation method comprising the following steps:
[0081] (1) 200 mL of 1.5 mol / L aluminum isopropoxide aqueous solution was first hydrolyzed at 84° C. and 500 rpm for 1.5 h, then the temperature was raised to 95° C., 40 mL of 1 mol / L nitric acid was added, 4.6 g of Li2CO3 and 17.9 g of MnCO3 were added after the first hydrolysis for 2 h, and the second hydrolysis was carried out at 95° C. for 22 h to obtain an alumina composite gel;
[0082] (2) 0.75 g of graphite and the alumina composite gel described in step (1) were mixed in a blue sand mill at a speed of 3000 rpm for 30 min, then dried at 70° C. for 3 h, extruded by a screw extruder, and then heated to 500° C. at a heating rate of 5° C. / min and calcined for 5 h to obtain a composite lithium adsorbent precursor;
[0083] (3) Activating the composite lithium adsorbent precursor of step (2) in 0.5 mol / L hydrochloric acid to obtain a composite lithium adsorbent.
[0084] Example 4
[0085] This embodiment provides a method for preparing a composite lithium adsorbent. Except that the "100 mL 1.5 mol / L aluminum isopropoxide aqueous solution" in step (1) is replaced by "100 mL 0.5 mol / L aluminum isopropoxide aqueous solution", other conditions are the same as those in Example 1.
[0086] Example 5
[0087] This embodiment provides a method for preparing a composite lithium adsorbent. Except that the "100 mL 1.5 mol / L aluminum isopropoxide aqueous solution" in step (1) is replaced by "100 mL 5 mol / L aluminum isopropoxide aqueous solution", other conditions are the same as those in Example 1.
[0088] Example 6
[0089] This embodiment provides a method for preparing a composite lithium adsorbent. Except that "4.6 g Li2CO3" in step (1) is replaced by "2.6 g Li2CO3", other conditions are the same as those in Example 1.
[0090] Example 7
[0091] This embodiment provides a method for preparing a composite lithium adsorbent. Except that "4.6 g Li2CO3" in step (1) is replaced by "7.5 g Li2CO3", other conditions are the same as those in Example 1.
[0092] Example 8
[0093] This embodiment provides a method for preparing a composite lithium adsorbent. Except that "0.5 g of graphite" in step (2) is replaced by "2 g of graphite", other conditions are the same as those in Example 1.
[0094] Example 9
[0095] This embodiment provides a method for preparing a composite lithium adsorbent. Except that the calcination temperature in step (2) is 120° C., other conditions are the same as those in Example 1.
[0096] Example 10
[0097] This embodiment provides a method for preparing a composite lithium adsorbent. Except that the calcination temperature in step (2) is 700° C., other conditions are the same as those in Example 1.
[0098] Comparative Example 1
[0099] This comparison provides a method for preparing a composite lithium adsorbent. Except that in step (1), no aluminum source solution is added and 4.6 g Li2CO3 and 17.9 g MnCO3 are directly mixed, other conditions are the same as those in Example 1.
[0100] Comparative Example 2
[0101] This comparison provides a method for preparing a composite lithium adsorbent. Except that 0.5 g of graphite is not added in step (2), other conditions are the same as those in Example 1.
[0102] Comparative Example 3
[0103] This comparison provides a method for preparing a composite lithium adsorbent, except that step (3) is not performed, other conditions are the same as those in Example 1.
[0104] Comparative Example 4
[0105] This comparative example provides a method for preparing a composite lithium adsorbent, the preparation method comprising the following steps:
[0106] (1) 100 mL of 1.5 mol / L aluminum isopropoxide aqueous solution was first hydrolyzed at 85° C. and a rotation speed of 260 rpm for 1.5 h, then heated to 95° C., and 30 mL of 1 mol / L nitric acid was added at the same time. After the first hydrolysis for 2 h, 17.9 g of MnCO3 was added, and the second hydrolysis was performed for 24 h, and then dried at 70° C. for 4 h, and then heated to 600° C. at a heating rate of 5° C. / min and calcined and kept at this temperature for 4 h to obtain a powder;
[0107] (2) 4.6 g of Li2CO3 and the powder of step (1) were mixed for 30 min, and then the temperature was raised to 600°C at a heating rate of 5°C / min, calcined and kept at this temperature for 4 h to obtain a composite lithium adsorbent.
[0108] The composite lithium adsorbents prepared in the above examples and comparative examples were characterized, and the characterization results are shown in Table 1.
[0109] Table 1
[0110]
[0111]
[0112] The composite lithium adsorbents prepared in the above embodiments and comparative examples were tested for lithium adsorption performance. The test method was as follows: 0.2 g of the composite lithium adsorbent was placed in 100 mL of a 0.1 mol / L lithium-containing solution (pH = 10 pure lithium solution), shaken for 24 h, and the lithium ion concentration in the solution before and after adsorption was determined by ICP, and the adsorption capacity was calculated. The test results are shown in Table 2.
[0113] Table 2
[0114]
[0115]
[0116] From Table 1 and Table 2, we can draw the following conclusions:
[0117] (1) The preparation method of the composite lithium adsorbent provided in Examples 1-3 of the present invention, the prepared composite lithium adsorbent has high porosity and high specific surface area, can achieve rapid adsorption in an aqueous environment, can reach adsorption equilibrium within 9 hours, and the saturated adsorption capacity in the lithium precipitation mother liquor is as high as 25 mg / g;
[0118] (2) From the comparison between Example 1 and Examples 4-5, it can be seen that when the amount of aluminum source added is too low, the amount of alumina gel is small, which leads to a higher lithium content in the material, and the lithium sites account for a large proportion after activation, so the adsorption capacity is large, but the stability of the composite lithium adsorbent material becomes poor and cannot be reused; when the amount of aluminum source added is too high, the amount of alumina gel is large, which leads to a lower lithium content in the material, and the lithium sites account for a small proportion after activation, so the adsorption capacity is small; from the comparison between Example 1 and Example 8, it can be seen that when too much pore-forming agent is added (increased from 2.4% to 9.73%), the pore-forming agent becomes carbon dioxide after calcination and escapes, leaving vacancies, and the pore structure of the prepared composite lithium adsorbent is richer, the adsorption rate becomes faster, but the material becomes brittle and the stability decreases;
[0119] (3) From the comparison between Example 1 and Examples 9-10, it can be seen that when the calcination end temperature is too low, the effective components in the material are reduced due to insufficient reaction, resulting in a low adsorption capacity of the prepared composite lithium adsorbent; when the calcination end temperature is too high, more side reactions occur due to sufficient reaction, resulting in a reduced effective component of the prepared composite lithium adsorbent and a lower adsorption capacity;
[0120] (4) It can be seen from the comparison between Example 1 and Comparative Example 1 and Comparative Example 4 that when the manganese lithium molecular sieve is directly prepared, because it is a powder material and is in full contact with the liquid, its adsorption performance is good, but it cannot be directly applied to the industrial adsorption and desorption device; when multiple mixing and calcination are used, the obtained composite lithium adsorbent has no lithium adsorption capacity;
[0121] (5) By comparing Example 1 with Comparative Examples 2-3, it can be seen that when the pore-forming agent is not added, the adsorption capacity of the prepared composite lithium adsorbent decreases due to the small specific surface area; when the acid solution activation is not performed, the lithium ions in the adsorbent are not removed, and there are no extra sites in the adsorbent to adsorb lithium, resulting in the prepared composite lithium adsorbent having almost no adsorption capacity.
[0122] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a composite lithium adsorbent, characterized in that: The preparation method comprises the following steps: (1) After the aluminum source solution is subjected to a first hydrolysis, a lithium source and a manganese source are added to perform a second hydrolysis to obtain an alumina composite gel; (2) mixing the pore-forming agent and the alumina composite gel of step (1) in a mass ratio of (0.1%-3%):1, and then drying, molding and calcining in sequence to obtain a composite lithium adsorbent precursor; (3) Activating the composite lithium adsorbent precursor in step (2) to obtain a composite lithium adsorbent.
2. The preparation method according to claim 1, characterized in that: The aluminum source in the aluminum source solution of step (1) includes any one of aluminum chloride, aluminum isopropoxide, triethylaluminum, triisobutylaluminum, diisobutylaluminum hydride and dimethylaluminum hydride, or a combination of at least two thereof.
3. The preparation method according to claim 2, characterized in that: The aluminum source in the aluminum source solution of step (1) is triethylaluminum or aluminum isopropoxide.
4. The preparation method according to claim 1, characterized in that: The concentration of the aluminum source solution in step (1) is 1.5-3.5 mol / L.
5. The preparation method according to claim 1, characterized in that: The temperature of the first hydrolysis in step (1) is 25-95°C.
6. The preparation method according to claim 5, characterized in that: The temperature of the first hydrolysis in step (1) is 50-90°C.
7. The preparation method according to claim 1, characterized in that: The first hydrolysis in step (1) is carried out under stirring conditions.
8. The preparation method according to claim 7, characterized in that: The rotation speed of the first hydrolysis in step (1) is 100-500 rpm.
9. The preparation method according to claim 1, characterized in that: Step (1) After the first hydrolysis for 1-2 hours, an acid solution is added.
10. The preparation method according to claim 9, characterized in that: The acid solution includes nitric acid and / or hydrochloric acid.
11. The preparation method according to claim 9, characterized in that: The concentration of the acid solution is 1-2 mol / L.
12. The preparation method according to claim 1, characterized in that: Step (1) After the first hydrolysis for 2-4 hours, the lithium source and the manganese source are added.
13. The preparation method according to claim 1, characterized in that: The lithium source in step (1) includes any one of lithium carbonate, lithium nitrate, lithium acetate, lithium oxalate, lithium chloride, lithium hydroxide or lithium sulfate, or a combination of at least two thereof.
14. The preparation method according to claim 13, characterized in that: The lithium source in step (1) is lithium hydroxide or lithium carbonate.
15. The preparation method according to claim 1, characterized in that: The manganese source in step (1) includes any one of manganese carbonate, manganese dioxide, potassium permanganate, manganese carbonate or manganese nitrate, or a combination of at least two thereof.
16. The preparation method according to claim 15, characterized in that: The manganese source in step (1) is manganese carbonate or manganese dioxide.
17. The preparation method according to claim 1, characterized in that: The molar ratio of the lithium source to the manganese source in step (1) is (0.6-1):
1.
18. The preparation method according to claim 1, characterized in that: The temperature of the second hydrolysis in step (1) is 70-95°C.
19. The preparation method according to claim 1, characterized in that: The second hydrolysis time in step (1) is 15-24 hours.
20. The preparation method according to claim 1, characterized in that: The pore-forming agent in step (2) includes any one of graphite, activated carbon, polyvinyl alcohol, polyvinyl chloride, calcium silicate or calcium carbonate, or a combination of at least two thereof.
21. The preparation method according to claim 20, characterized in that: The pore-forming agent in step (2) is graphite or calcium carbonate.
22. The preparation method according to claim 1, characterized in that: The mixing time in step (2) is 20-60 minutes.
23. The preparation method according to claim 1, characterized in that: The drying temperature in step (2) is 50-100°C.
24. The preparation method according to claim 23, characterized in that: The drying temperature in step (2) is 60-70°C.
25. The preparation method according to claim 1, characterized in that: The drying time in step (2) is 3-10 hours.
26. The preparation method according to claim 1, characterized in that: The molding in step (2) is extrusion molding.
27. The preparation method according to claim 1, characterized in that: The heating rate of the calcination in step (2) is 4-8°C / min.
28. The preparation method according to claim 1, characterized in that: The calcination temperature in step (2) is 120-600°C.
29. The preparation method according to claim 28, characterized in that: The calcination temperature in step (2) is 400-600°C.
30. The preparation method according to claim 1, characterized in that: The calcination holding time in step (2) is 4-6 hours.
31. The preparation method according to claim 1, characterized in that: The activation treatment in step (3) is carried out in an acid solution.
32. The preparation method according to claim 31, characterized in that: The acid solution includes nitric acid and / or hydrochloric acid.
33. The preparation method according to claim 31, characterized in that: The concentration of the acid solution is 0.1-0.5 mol / L.
34. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) After a first hydrolysis of a 1.5-3.5 mol / L aluminum source solution at 25-95° C. and a rotation speed of 100-500 rpm for 1-2 hours, an acid solution at a concentration of 1-2 mol / L is added, and after the first hydrolysis for 2-4 hours, a lithium source and a manganese source are added, and a second hydrolysis is performed at 70-95° C. for 15-24 hours to obtain an alumina composite gel; The molar ratio of the lithium source to the manganese source is (0.6-1):1; (2) mixing the pore-forming agent and the alumina composite gel of step (1) for 20-60 minutes, drying at 50-100°C for 3-10 hours, extruding and molding, and then heating to 120-600°C at a heating rate of 4-8°C / min, calcining and keeping the temperature for 4-6 hours to obtain a composite lithium adsorbent precursor; The mass ratio of the pore-forming agent to the alumina composite gel in step (1) is (0.1%-3%):1; (3) Activating the composite lithium adsorbent precursor in step (2) in an acid solution with a concentration of 0.1-0.5 mol / L to obtain a composite lithium adsorbent.
35. A composite lithium adsorbent, characterized in that: The method is prepared by any one of claims 1 to 34.
36. The composite lithium adsorbent according to claim 35, characterized in that The pore volume of the composite lithium adsorbent is 0.270-0.300 m 3 / g.
37. The composite lithium adsorbent according to claim 35, characterized in that The specific surface area of the composite lithium adsorbent is 150-160 m 2 / g.