A method and device for growing tellurium dioxide single crystal

Through the multi-crystal growth method of heating and uniform rotation, it solves the problems of high equipment and low output in the existing tellurium dioxide single crystal growth technology, and achieves the growth and production of high-quality, low-defect large-sized tellurium dioxide single crystals. Cost reduction.

CN116103746BActive Publication Date: 2024-10-01FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211584868.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-01
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Existing tellurium dioxide single crystal growth technologies have limitations such as the pull-up method and the crucible-down method. The pull-up method requires high-end equipment and the products are irregular. The crucible drop-down method has high costs and low output, making it difficult to meet the needs of industrial production.

Method used

The multi-root crystal growth method of heating and uniform rotation is adopted. By setting up multiple crucibles to rotate at a uniform speed between the high temperature zone and the low temperature zone, the temperature gradient and rotation speed are controlled to overcome the problems of single root growth and high cost.

Benefits of technology

It achieves the growth of high-quality, low-defect tellurium dioxide single crystals, improves the yield and output, reduces production costs, and can grow large-sized high-quality single crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116103746B_ABST
    Figure CN116103746B_ABST
Patent Text Reader

Abstract

The present application discloses a method for growing a tellurium dioxide single crystal and a growing device thereof. The crystal rotates at a uniform speed during the growth process and multiple crystals grow simultaneously. The method overcomes the defects such as encapsulation and stripes in the crystal caused by the single cooling process of the tellurium dioxide crystal growth by the crucible descent method, and also overcomes the disadvantages of only single crystal growth and relatively high cost. The obtained tellurium dioxide single crystal has high quality, few defects, high yield, is easy to produce and has low cost, and can grow high-quality single crystals with a size of φ60mm*80mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a method and device for growing a tellurium dioxide single crystal, and belongs to the field of crystal growth. Background Art

[0002] Tellurium dioxide crystal is an acousto-optic crystal with excellent performance. The crystal is currently mainly used in acousto-optic modulators, acousto-optic deflectors, acousto-optic modulators, etc. It is also used to study neutrinos and dark matter.

[0003] At present, there are two main technologies for growing tellurium dioxide single crystals: the Czochralski method and the crucible descent method. The Czochralski method requires inert gas during the pulling process and has high requirements for the pulling furnace. The grown crystals are irregular cylinders with low utilization rate and cannot meet the required size of the device.

[0004] Compared with the Czochralski method, the crucible descent method can avoid raw material volatilization and toxic pollution, and is easier to grow large-sized single crystals with a high yield rate. Chinese patent CN 1306074C has reported this method, but due to its single descent process and single root growth, low output and high cost, it is not suitable for large-scale production in enterprises. Summary of the invention

[0005] According to one aspect of the present application, a method for growing a tellurium dioxide single crystal and a growth device thereof are provided. The temperature rise process and the growth process are rotated at a uniform speed, and multiple crystals are grown simultaneously to solve the defects such as encapsulation and stripes in the crystal caused by a single cooling process during the cooling process, and also overcome the disadvantage that only a single crystal can be grown before and the cost is relatively high. The tellurium dioxide single crystal obtained by this method has high quality, few defects, high yield, is easy to produce and has low cost, and can grow a high-quality single crystal of φ60mm*80mm.

[0006] According to a first aspect of the present application, a method for growing a tellurium dioxide single crystal is provided.

[0007] A method for growing a tellurium dioxide single crystal comprises the following steps:

[0008] (S1) placing a tellurium dioxide seed crystal at the bottom of a crucible, adding bulk tellurium dioxide, and sealing;

[0009] (S2) The crucible rotates at a constant speed, and the speed of the constant rotation is set to R 1 ; Set the growth temperature to T 1 , the holding time is t 1 ;

[0010] Among them, R 1 =20~35rad / m;

[0011] T 1 =720~750℃;

[0012] t 1 =4~15h;

[0013] (S3) The crucible rotates and descends at a uniform speed, and the speed of uniform rotation is set to R 2 ; Set the descent rate to v and the descent time to t 2 ; Set the temperature gradient to GT;

[0014] Among them, R 2 =8~20rad / m;

[0015] v = 0.2 ~ 0.8 mm / h;

[0016] t 2 =120~280h;

[0017] GT=15-35℃ / cm.

[0018] (S4) stopping the descending and rotating, cooling to room temperature, and obtaining the tellurium dioxide single crystal.

[0019] Optionally, in step (S1), N crucibles are arranged in parallel, where N=1 to 5, which is a positive integer.

[0020] Optionally, N = 1, 2 or 3. By arranging multiple crucibles, different crucibles are on the same horizontal line and keep the temperature field consistent, and the links between the crucibles are special high-temperature resistant metal twisted parts, multiple crystals can be grown simultaneously, thereby increasing output and reducing costs.

[0021] Optionally, in step (S1), the tellurium dioxide seed crystal is in the

[110] direction.

[0022] In the present invention, the shape of the seed crystal can be selected according to the shape of the selected crystal. If a cylindrical single crystal needs to be grown, the seed crystal is cylindrical, such as with a size of Φ50mm×5mm. If a cylindrical conical single crystal is needed, the seed crystal is processed into a cone, such as with a bottom diameter of Φ20mm and a height of 5mm.

[0023] Optionally, in step (S2), the uniform rotation speed R 1 Greater than R 2 .

[0024] Optionally, in step (S2), R 1 =20~30rad / m;

[0025] T 1 =730-740℃;

[0026] t 1 =6~12h.

[0027] Optionally, the uniform rotation speed R 1Independently selected from any value among 20rad / m, 22rad / m, 24rad / m, 25rad / m, 26rad / m, 28rad / m, 30rad / m, 32rad / m, 34rad / m, 35rad / m or any range therebetween.

[0028] Optionally, the growth temperature T 1 Independently selected from any value of 720°C, 730°C, 732°C, 734°C, 735°C, 736°C, 738°C, 740°C, 742°C, 744°C, 745°C, 746°C, 748°C, 750°C, or any range therebetween.

[0029] Optionally, the holding time t 1 Independently selected from any value of 4h, 6h, 8h, 10h, 12h, 14h, 15h, or a range between any two of them.

[0030] Optionally, in step (S2), the growth temperature T is reached by program heating. 1 The rate of the programmed temperature increase is 10 to 20°C / h.

[0031] Optionally, the rate of the programmed temperature increase is independently selected from any value of 10°C / h, 12°C / h, 14°C / h, 15°C / h, 16°C / h, 18°C / h, 20°C / h, or any range therebetween.

[0032] Optionally, in step (S3), R 2 =8~15rad / m;

[0033] v = 0.3-0.6 mm / h;

[0034] t 2 =125~250h;

[0035] GT=20-30℃ / cm.

[0036] Optionally, the uniform rotation speed R 2 Independently selected from any value among 8rad / m, 10rad / m, 12rad / m, 14rad / m, 15rad / m, 16rad / m, 18rad / m, 20rad / m, or any range therebetween.

[0037] Optionally, the descending rate v is independently selected from any value among 0.2 mm / h, 0.3 mm / h, 0.4 mm / h, 0.5 mm / h, 0.6 mm / h, 0.7 mm / h, 0.8 mm / h, or any range therebetween.

[0038] Optionally, the fall time t 2 Any value independently selected from 120h, 125h, 140h, 150h, 160h, 180h, 200h, 220h, 240h, 260h, 280h, or a range between any two of the values.

[0039] Optionally, the temperature gradient GT is independently selected from any value among 15°C / cm, 18°C / cm, 20°C / cm, 22°C / cm, 24°C / cm, 25°C / cm, 26°C / cm, 28°C / cm, 30°C / cm, 32°C / cm, 34°C / cm, 35°C / cm, or any range therebetween.

[0040] Optionally, in step (S4), the cooling rate is 20 to 40°C / h.

[0041] Optionally, the cooling rate is independently selected from any value of 20°C / h, 22°C / h, 25°C / h, 28°C / h, 30°C / h, 32°C / h, 35°C / h, 38°C / h, 40°C / h or any range therebetween.

[0042] Optionally, the size of the tellurium dioxide single crystal is φ20~60mm*50~80mm.

[0043] Optionally, the size of the tellurium dioxide single crystal is φ30-60 mm*60-80 mm.

[0044] Optionally, the tellurium dioxide single crystal has a size of φ50 mm*70 mm.

[0045] Optionally, the tellurium dioxide single crystal has a size of φ30 mm*75 mm.

[0046] Optionally, the tellurium dioxide single crystal has a size of φ60 mm*80 mm.

[0047] Optionally, the size of the tellurium dioxide single crystal may be φ60mm*80mm. The growing method of the present invention can not only obtain large-sized crystals, but also overcome defects such as wrapping and stripes in the crystals.

[0048] According to a second aspect of the present application, a tellurium dioxide single crystal growth device is provided.

[0049] A tellurium dioxide single crystal growth device, the growth device comprising a high temperature zone, a low temperature zone, and N crucible systems;

[0050] Below the high temperature zone is a low temperature zone, and there is a gap between the high temperature zone and the low temperature zone;

[0051] Each crucible system is arranged in parallel;

[0052] The N crucible systems can move up and down in the cavity enclosed by the high temperature zone and the low temperature zone;

[0053] Each crucible system includes a crucible, and a quartz base, a support column and a rotating system are sequentially arranged below the crucible;

[0054] The rotating system drives the crucible to rotate through the supporting column and the quartz base;

[0055] Wherein, N=1 to 5, which is a positive integer.

[0056] Optionally, N=1, 2 or 3.

[0057] In the present invention, multiple crucible systems are provided to achieve simultaneous growth of multiple crystals, thereby increasing output and reducing costs.

[0058] Optionally, the gap may be cooled by air cooling or water cooling.

[0059] In the present invention, there is a certain gap between the high temperature zone and the low temperature zone, which increases the temperature gradient required for crystal growth and makes it easy for the crystal to grow. The hollow area between the high temperature zone and the low temperature zone is cooled by air or water to control the temperature.

[0060] Optionally, the crucible is a platinum crucible;

[0061] The crucible is divided into four parts, the bottom is the seed crystal area, the middle is the conical area, the upper part is the equal diameter area, and the top is the cover;

[0062] The crucible is cylindrical or square.

[0063] In the present invention, the shape of the crucible corresponds to the shape of the grown crystal, and the corresponding seed crystal shape is selected accordingly.

[0064] Optionally, the size of the crucible is φ20~60mm*55~130mm.

[0065] Optionally, the size of the crucible is φ50mm*120mm.

[0066] In the present invention, the shape and size of the crucible can be designed accordingly according to the shape and size of the crystal to be grown.

[0067] Optionally, the high temperature zone, the bottom of the quartz base, and the low temperature zone are all provided with thermocouples.

[0068] In the present invention, the temperature is controlled by a thermocouple so that the high temperature zone, the bottom of the quartz base, and the low temperature zone reach the set temperature.

[0069] Optionally, the support column is a quartz tube;

[0070] The rotating system includes a motor, a fixing and connecting device, etc. The rotating system is also provided with a speed regulator, and the rotating speed of the crucible is adjusted by the rotating system.

[0071] Optionally, a cover is also provided on the top of the high temperature zone.

[0072] As a preferred embodiment, the method for growing a tellurium dioxide single crystal includes pressing raw material powder, sealing and welding a crucible, loading a furnace, a uniform rotation heating process, a crystal uniform rotation growth process, and an annealing process;

[0073] (1) Pressing the raw material powder to press the high-purity tellurium dioxide powder into blocks;

[0074] (2) The crucible is sealed by welding, a seed crystal is placed at the bottom of the crucible, and then a block of tellurium dioxide is placed, and a lid is put on and sealed by welding;

[0075] (3) Loading multiple crucibles into the furnace, placing multiple sealed crucibles on a quartz base and raising them to the crystal growth area;

[0076] (4) During the heating process of uniform rotation, a heating program is set to increase the temperature, and the speed is set to make the crucible rotate at a uniform speed;

[0077] (5) During the crystal growth process, the crucible is kept warm for a period of time and then allowed to rotate downward at a constant speed.

[0078] (6) During the annealing process, when the crucible drops to a certain size, stop descending and rotating, set a cooling program, cool it down to room temperature, take out the crucible, and perform subsequent processing on the crystal.

[0079] Optionally, the crucible descending furnace used for growth is divided into three sections for temperature control, and there is a certain gap between the high temperature zone and the low temperature zone, which increases the temperature gradient required for crystal growth and makes it easier for crystals to grow.

[0080] Optionally, the heating process is to raise the crucible to the high temperature area and then keep rotating at a constant speed, heating at 60°C / h to keep the temperature in the high temperature area at 780°C. The rotation speed can be faster than the growth process and maintained at 20-30rad / m. After the crystal growth is completed, the annealing process is cooled at 20-40°C / h to keep the three-stage temperature control program synchronized and drop to room temperature.

[0081] Optionally, when the crucible is in the high temperature zone, the optimal temperature of the bottom of the crucible is 730-740° C., and the temperature is kept for 6 to 12 hours.

[0082] The beneficial effects of this application include:

[0083] The method and device for growing a tellurium dioxide single crystal provided in the present application not only stabilize the longitudinal temperature gradient during crystal growth, but also make the lateral temperature gradient tend to be balanced, so that the crystal can be easily crystallized during the growth process, and a tellurium dioxide crystal with good optical quality, high purity and large size can be obtained. At the same time, the present invention can grow multiple crystals at the same time, thereby increasing production and reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0084] Figure 1 This is a schematic diagram of the structure of the equipment used for growing tellurium dioxide single crystals of the present invention.

[0085] Figure 2 This is a photograph of the tellurium dioxide crystal grown in Example 1.

[0086] Figure 3 This is a photograph of the tellurium dioxide crystal grown in Example 2.

[0087] Figure 4 This is a photograph of the tellurium dioxide crystal grown in Comparative Example 1.

[0088] Figure 5 This is a photograph of the tellurium dioxide crystal grown in Comparative Example 2.

[0089] Figure 1 List of reference numerals:

[0090] 1. Temperature control thermocouple 2. Platinum crucible 3. Quartz base

[0091] 4. Hollow area 5. Quartz tube 6. Rotation system. DETAILED DESCRIPTION

[0092] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0093] Unless otherwise specified, the raw materials in the examples of the present application are purchased through commercial channels. Unless otherwise specified, the test methods all adopt conventional methods, and the instrument settings all adopt the settings recommended by the manufacturer.

[0094] Among them, tellurium dioxide powder was purchased from Hangzhou Kaiyada Semiconductor Materials Co., Ltd. with a purity of 5N.

[0095] Figure 1 The schematic diagram of the structure of the equipment used for the growth of tellurium dioxide single crystals of the present invention. The equipment is composed of a furnace cover, a high temperature zone, and a low temperature zone from top to bottom. A hollow area 4 is provided between the high temperature zone and the low temperature zone, and the area can be cooled by air cooling or water cooling. For example, the temperature gradient can be adjusted by ventilation during air cooling. The upper and lower parts of the high temperature zone are both provided with temperature-controlling thermocouples 1, and the low temperature zone is also provided with thermocouples to accurately control the set temperature. Heating is performed by nickel-chromium wire.

[0096] In the crucible system, the base of the platinum crucible 2 is a quartz base 3, a fixed thermocouple is provided at the bottom of the base, the support column is a quartz tube 5, and a rotating system 6 is provided at the bottom of the quartz tube, and the rotating speed is adjustable. The rotating system includes a rotating motor and a speed regulator, and drives the platinum crucible 2 to rotate through the quartz tube 5 and the quartz base 3.

[0097] The crucible system can move up and down in the cavity enclosed by the high temperature zone and the low temperature zone. Multiple crucible systems can be set in parallel. Figure 1 Three are shown.

[0098] Example 1

[0099] The method for preparing the tellurium dioxide crystal of this embodiment comprises the following steps:

[0100] Take 850 g of commercially available tellurium dioxide powder with a purity of 5N, and press it into blocks using a tablet press at a pressure of 0.8 MPa, while keeping it dry during the process.

[0101] First, grind the seed crystal in the

[110] direction into a Φ50mm×5mm cylinder and place it in a platinum crucible made by Wuxi Interpai Platinum Co., Ltd. The crucible is cylindrical, with a diameter of 50mm, a height of 120mm, and a wall thickness of 0.2mm. Then put the pressed block tellurium dioxide into the cylindrical crucible 2, fill the gap with tellurium dioxide powder, and then cover it with a lid and use a spot welder to weld and seal it.

[0102] The three crucibles are sealed at the same time, the quartz tube 5 is lowered, placed on the quartz base 3, and then raised to the position of the high temperature zone.

[0103] Then set the heating program, with the top set to 780°C, the middle set to 700°C, the bottom set to 450°C, and the heating rate set to 18°C / h. Then adjust the rotating system 6 to make the rotation speed 25rad / m, wait for the program to heat up to the set temperature, adjust the crucible position, make the bottom temperature of the crucible around 740°C, not too high, and keep warm for 12 hours.

[0104] After the insulation was completed, the crucible began to descend at a descending rate of 0.3 mm / h, and at the same time the rotation speed was changed from 25 rad / m to 15 rad / m, so that the temperature gradient was maintained at 25°C / cm, and the temperature gradient was adjusted by ventilation in the central control area.

[0105] When the crucible has been descending for 235h, stop descending and rotating, set the cooling program, and set the cooling rate to 25℃ / h, so that the three-stage temperature-controlled thermocouples can be cooled synchronously until the temperature drops to room temperature and stop.

[0106] After the temperature drops to room temperature, take out the crucible, cut the crucible with scissors, and carefully take out the crystal. Figure 2The picture shown is a photo of the grown tellurium dioxide crystal. It can be seen that it is cylindrical with a size of Φ50mm*70mm. The crystal is pure without defects such as wrapping and stripes.

[0107] Example 2

[0108] Take 350 g of commercially available tellurium dioxide powder with a purity of 5N, and press it into blocks using a tablet press at a pressure of 0.8 MPa, while keeping it dry during the process.

[0109] First, grind the seed crystal in the

[110] direction into a Φ30mm×5mm cylinder and place it in a platinum crucible made by Wuxi Interpai Platinum Co., Ltd. The crucible is cylindrical, with a diameter of 30mm, a height of 140mm, and a wall thickness of 0.2mm. Then place the pressed block tellurium dioxide into the cylindrical crucible 2, fill the gap with tellurium dioxide powder, and then cover it with a lid and use a spot welder to weld and seal it.

[0110] The three crucibles are sealed at the same time, the quartz tube 5 is lowered, placed on the quartz base 3, and then raised to the position of the high temperature zone.

[0111] Then set the heating program, with the top set to 750°C, the middle set to 720°C, the bottom set to 430°C, and the heating rate set to 18°C / h. Then adjust the rotating system 6 to make the rotation speed 20rad / m, wait for the program to heat up to the set temperature, adjust the crucible position, make the bottom temperature of the crucible around 735°C, not too high, and keep warm for 6 hours.

[0112] After the insulation is completed, the crucible begins to descend at a descending rate of 0.45 mm / h, and at the same time the rotation speed is changed from 20 rad / m to 10 rad / m, so that the temperature gradient is maintained at 25°C / cm, and the temperature gradient is adjusted by circulating water in the central control area.

[0113] When the crucible has been descending for 250h, stop descending and rotating, set a cooling program with a cooling rate of 20℃ / h, and make the three-stage temperature-controlled thermocouples cool synchronously until the temperature drops to room temperature and stops.

[0114] After the temperature drops to room temperature, take out the crucible and carefully cut it with scissors. The photo of the grown tellurium dioxide crystal is as follows: Figure 3 As shown, it can be seen that it is cylindrical, with a size of Φ30mm*75mm, and the crystal is pure without defects such as wrapping and stripes.

[0115] Comparative Example 1

[0116] 560 g of commercially available tellurium dioxide powder with a purity of 5N was taken and pressed into blocks using a tablet press at a pressure of 0.8 MPa, while keeping it dry during the process.

[0117] First, grind the seed crystal in the

[110] direction into a Φ20mm×5mm cone and place it in a platinum crucible made by Wuxi Interpai Platinum Co., Ltd. The crucible is a cylindrical cone with a diameter of 50mm, a cylindrical part height of 110mm, a conical part height of 30mm, and a wall thickness of 0.2mm. Then place the pressed block tellurium dioxide into the cylindrical cone crucible 2, fill the gap with tellurium dioxide powder, and then cover it with a lid and use a spot welder to weld and seal it.

[0118] The three crucibles are sealed at the same time, the quartz tube 5 is lowered, placed on the quartz base 3, and then raised to the position of the high temperature zone.

[0119] Then set the heating program, with the top set to 780℃, the middle set to 700℃, and the bottom set to 400℃. The heating rate is 18℃ / h. Wait for the program to heat up to the set temperature. Adjust the crucible position so that the temperature at the bottom of the crucible is around 735℃, not too high, and keep warm for 6 hours.

[0120] After the insulation is completed, the crucible begins to descend at a descending rate of 0.45 mm / h to keep the temperature gradient at 25°C / cm, and the temperature gradient is adjusted by circulating water in the central control area.

[0121] When the crucible has been descending for 250h, stop descending, set the cooling program, and set the cooling rate to 20℃ / h, so that the three-stage temperature-controlled thermocouples can be cooled synchronously until the temperature drops to room temperature and stop.

[0122] After the temperature drops to room temperature, take out the crucible and carefully cut it with scissors. The photo of the grown tellurium dioxide crystal is as follows: Figure 4 As shown, it can be seen that it is a cylindrical cone with a size of Φ50mm*65mm. The quality is good at about 20mm height after the crystal is equal in diameter, and the rest of the part has defects such as wrapping, stripes, and polycrystalline.

[0123] Comparative Example 2

[0124] 580 g of commercially available tellurium dioxide powder with a purity of 5N was taken and pressed into blocks using a tablet press at a pressure of 0.8 MPa, while keeping it dry during the process.

[0125] First, grind the seed crystal in the

[110] direction into a Φ30mm×5mm cylinder and place it in a platinum crucible made by Wuxi Interpai Platinum Co., Ltd. The crucible is a cylindrical cone with a diameter of 50mm, a cylindrical part height of 110mm, a conical part height of 30mm, and a wall thickness of 0.2mm. Then put the pressed block tellurium dioxide into the cylindrical crucible 2, fill the gap with tellurium dioxide powder, and then cover it with a lid and use a spot welder to weld and seal it.

[0126] The three crucibles are sealed at the same time, the quartz tube 5 is lowered, placed on the quartz base 3, and then raised to the position of the high temperature zone.

[0127] Then set the heating program, with the top set to 750°C, the middle set to 720°C, the bottom set to 400°C, and the heating rate set to 18°C / h. Then adjust the rotating system 6 to make the rotation speed 15rad / m, wait for the program to heat up to the set temperature, adjust the crucible position, make the bottom temperature of the crucible around 735°C, not too high, and keep warm for 6 hours.

[0128] After the insulation is completed, the crucible begins to descend at a descending rate of 0.45 mm / h, and at the same time the rotation speed is changed from 15 rad / m to 25 rad / m, so that the temperature gradient is maintained at 25°C / cm, and the temperature gradient is adjusted by circulating water in the central control area.

[0129] When the crucible has been descending for 250h, stop descending and rotating, set a cooling program with a cooling rate of 20℃ / h, and make the three-stage temperature-controlled thermocouples cool synchronously until the temperature drops to room temperature and stops.

[0130] After the temperature drops to room temperature, take out the crucible and carefully cut the crucible with scissors. Figure 5 As shown, it is a photo of the grown tellurium dioxide crystal. It can be seen that it is cylindrical with a size of Φ50mm*60mm. The shoulder section and a small section between the equal diameters of the crystal are relatively pure, while the rest has defects such as polycrystalline, impurity inclusions, and growth stripes.

[0131] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for growing a tellurium dioxide single crystal, characterized in that: The following steps are involved: (S1) placing a tellurium dioxide seed crystal at the bottom of a crucible, adding bulk tellurium dioxide, and sealing; (S2) The crucible rotates at a constant speed, and the speed of the constant rotation is set to R1; the growth temperature is set to T1, and the holding time is set to t1; Among them, R1=20~35rad / m; T1=720~750℃; t1=4~15h; (S3) The crucible rotates and descends at a uniform speed, and the speed of the uniform rotation is set to R2; the descending rate is set to v, the descending time is set to t2; and the temperature gradient is set to GT; Among them, R2=8~20rad / m; v = 0.2 ~ 0.8 mm / h; t2=120~280h; GT = 15 ~ 35 ° C / cm; (S4) stopping the descending and rotating, cooling to room temperature, and obtaining the tellurium dioxide single crystal.

2. The growth method according to claim 1, characterized in that In step (S1), N crucibles are arranged in parallel, where N=1-5, which is a positive integer.

3. The growth method according to claim 1, characterized in that: In step (S1), the tellurium dioxide seed crystal is in the [110] direction.

4. The growth method according to claim 1, characterized in that: In step (S2), the speed R1 of the uniform rotation is greater than R2.

5. The growth method according to claim 1, characterized in that: In step (S2), R1=20~30rad / m; T1=730-740℃; t1=6~12h.

6. The growth method according to claim 1, characterized in that: In step (S2), the growth temperature T1 is reached by programmed temperature increase, and the rate of the programmed temperature increase is 10-20°C / h.

7. The growth method according to claim 1, characterized in that: In step (S3), R2=8~15rad / m; v = 0.3 ~ 0.6 mm / h; t2=125~250h; GT=20-30℃ / cm.

8. The growth method according to claim 1, characterized in that: In step (S4), the cooling rate is 20-40°C / h.

9. The growth method according to claim 1, characterized in that: The size of the tellurium dioxide single crystal is φ20~60mm*50~80mm.

10. The growth method according to claim 1, characterized in that: The growth method uses the following growth device; The growth device includes a high temperature zone, a low temperature zone, and N crucible systems; Below the high temperature zone is a low temperature zone, and there is a gap between the high temperature zone and the low temperature zone; Each crucible system is arranged in parallel; The N crucible systems can move up and down in the cavity enclosed by the high temperature zone and the low temperature zone; Each crucible system includes a crucible, and a quartz base, a support column and a rotating system are sequentially arranged below the crucible; The rotating system drives the crucible to rotate through the supporting column and the quartz base; Among them, N=1~5, which is a positive integer.

11. The growth method according to claim 10, characterized in that: The gap can be cooled by air cooling or water cooling.

12. The growth method according to claim 10, characterized in that: The crucible is a platinum crucible; The crucible is divided into four parts, the bottom is the seed crystal area, the middle is the conical area, the upper part is the equal diameter area, and the top is the cover; The crucible is cylindrical or square.

13. The growth method according to claim 10, characterized in that: The size of the crucible is φ20~60mm *55~130mm.

14. The growth method according to claim 10, characterized in that: The high temperature zone and the low temperature zone are both provided with thermocouples.

15. The growth method according to claim 10, characterized in that: The support column is a quartz tube; The rotating system comprises a motor, fixing and connecting devices.