A coordination polymer material and its preparation method and application
By developing a coordination polymer material [Cd(1,3-bdc)(3,3'-tpcb)0.5], it can adsorb and collect moisture in the air in a low-humidity environment, and use solar collectors to generate liquid water. It solves the problem of low efficiency of existing technology in low-humidity environments and achieves the effect of small-scale portable air water extraction.
Patent Information
- Application Number
- CN202211634986.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-19
AI Technical Summary
The existing adsorption air water extraction technology has low efficiency in low-humidity environments, and the adsorbent performance is insufficient, making it difficult to effectively utilize water resources in the atmosphere.
Develop a coordination polymer material [Cd(1,3-bdc)(3,3'-tpcb)0.5], which generates a material with tiny pores through photocatalytic reaction, adsorbs moisture in the air in a low-humidity environment, and Solar collectors are used to evaporate and condense the adsorbed water into liquid water.
It can quickly adsorb and collect liquid water in a low-humidity environment of 20%-30%, realizing small-scale portable air water extraction. The preparation method is simple, the operation is repeatable, and the yield is high.
Smart Images

Figure CN116120573B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new materials, and in particular relates to a coordination polymer material which can be used for extracting water from the air in a decentralized, small-scale and portable manner in low-humidity areas, and a preparation method thereof. Background Art
[0002] Freshwater resources are the most important natural resources and the basis of all biological life activities. The freshwater resources that humans can actually use are quite limited.
[0003] The water vapor content in the air is large, renewable and clean. It is estimated that the amount of water in the air is 12.9×10 12 m 3 . However, the fresh water resources in the atmosphere have not been fully developed and utilized. In theory, the use of adsorbents and the adsorption air water extraction technology can adsorb water vapor in the atmosphere, and evaporate from the adsorbent driven by solar energy, lowering its dew point temperature, condensing the water vapor into liquid water, and converting it into fresh water that can be used by people. Adsorption air water extraction is a highly promising, flexible, convenient and low-energy way of extracting water.
[0004] In the adsorption-based air water extraction technology, the performance of the adsorbent is a key factor. High-performance adsorbents can significantly improve the efficiency of water extraction. Coordination polymer materials are one of the effective porous materials. Compared with traditional adsorption materials such as zeolite, silica gel, and molecular sieves, they have unique advantages such as controllable and adjustable hydrophilicity and low desorption and regeneration temperature. The research and development of new porous coordination polymer materials has gradually become a hot topic in the field of air water extraction. Summary of the invention
[0005] The present invention provides a coordination polymer material and a preparation method and application thereof. The coordination polymer material of the present invention can quickly absorb moisture in the air in a low humidity environment with an air humidity of 20%-30%. The high temperature generated by the solar collector causes the adsorbed water to evaporate from the coordination polymer lattice and condense into liquid water, thereby realizing small-scale air water extraction.
[0006] The coordination polymer material of the present invention is [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n , wherein 3,3'-tpcb is 1,2,3,4-tetra(3-pyridyl)cyclobutane, 1,3-bdc is 1,3-phthalate, and n is the number of repeating units, which is any positive integer.
[0007] Among them, the structural formulas of 1,2,3,4-tetra(3-pyridyl)cyclobutane and 1,3-phthalate are:
[0008]
[0009] 1,2,3,4-Tetra(3-pyridyl)cyclobutane
[0010]
[0011] The coordination polymer material of the present invention is a crystalline inorganic-organic hybrid material belonging to the triclinic system. The space group and unit cell parameters are α=112.88(3)°, β=90.29(3)°, γ=103.76(3)°.
[0012] The preparation method of the coordination polymer material of the present invention comprises the following steps:
[0013] Step 1: Place 1,2-di(3-pyridyl)ethylene, 1,3-phthalic acid, cadmium nitrate tetrahydrate and deionized water in a polytetrafluoroethylene reactor, seal the reactor, and react under high temperature and high pressure. After the reaction is completed, slowly cool to room temperature to obtain colorless block crystals [Cd(1,3-bdc)(3,3'-bpe)] n , filter, wash, dry and collect block crystals.
[0014] In step 1, the structural formula of 1,2-di(3-pyridyl)ethylene is as follows:
[0015]
[0016] In step 1, bulk crystals [Cd(1,3-bdc)(3,3'-bpe)] n The unit cell parameters are: α=114.07(3)°, β=91.09(3)°, γ=102.82(3)°.
[0017] Step 2: The bulk crystals obtained in step 1 are placed under sunlight for photocatalytic cycloaddition reaction to generate [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n The unit cell parameters are: α=64.85(3)°, β=87.73(3)°, γ=75.14(3)°.
[0018] Step 3: Heat the colorless block crystals obtained in step 2 to 120°C to remove the water molecules in the pores to obtain the coordination polymer material [Cd(1,3-bdc)(3,3'-tpcb)0.5 ] n .
[0019] In [Cd(1,3-bdc)(3,3'-bpe)] n In the structure, adjacent olefinic bonds are arranged in parallel, and the distance between olefinic bonds is This is consistent with the theory of olefin photocycloaddition proposed by Schmidt: the olefin bonds in adjacent olefin molecules must be arranged in parallel, and the distance between adjacent olefin bonds must be within Olefins can show photoreactivity. Various atoms are arranged in an orderly and regular manner, tightly packed, and the gaps between atoms are small. Coordination polymers [Cd(1,3-bdc)(3,3'-bpe)] n It does not absorb water. n When placed under sunlight, two adjacent 1,2-di(3-pyridyl)ethylenes undergo an addition reaction to generate 1,2,3,4-tetra(3-pyridyl)cyclobutane (as shown below). After the photocatalytic addition reaction, the atoms are significantly displaced, the two adjacent ethylene molecules are close to each other, and tiny gaps appear in the molecules (the gaps account for about 4% of the coordination polymer unit cell). The material absorbs water molecules in the air and forms hydrogen bonds with the water molecules. The bond lengths of the two hydrogen bonds are: and
[0020]
[0021] The application of the coordination polymer material of the present invention is to be used as an adsorption material in an air water extraction device to achieve adsorption and collection of liquid water from the air.
[0022] In the present invention, the coordination polymer material [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n When placed in a low humidity environment with an air humidity of 20%-30% for 10 minutes, it can absorb moisture in the environment and generate [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n By heating with solar collectors, the water adsorbed by the coordination polymer evaporates and condenses into liquid water, thus realizing small-scale air circulation water collection for households.
[0023] The preparation method of the invention has simple operation, good repeatability and high product yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 [Cd(1,3-bdc)(3,3'-bpe)] n Crystal structure diagram.
[0025] Figure 2 [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n Crystal structure diagram.
[0026] Figure 3 [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n Crystal structure diagram. DETAILED DESCRIPTION
[0027] Non-limiting examples are described below:
[0028] 1. [Cd(1,3-bdc)(3,3'-bpe)] n Synthesis
[0029] 1.82g (10mmol) of 1,2-di(3-pyridyl)ethylene, 1.66g (10mmol) of 1,3-phthalic acid, 3.08g (10mmol) of cadmium nitrate tetrahydrate and 50mL of deionized water were placed in a 100mL polytetrafluoroethylene reactor; the reactor was sealed and placed in a constant temperature drying oven at 170°C for 12 hours of high temperature and high pressure reaction; after the reaction was completed, the reaction mixture was slowly cooled to room temperature to obtain colorless block crystals, which were filtered, washed, dried and collected. Yield: 3.31g, yield: 72%.
[0030] [Cd(1,3-bdc)(3,3'-bpe)] n Some crystallographic parameters: C 20 H 14 CdN2O4,M r =458.74,triclinic, α=114.07(3)°, β=91.09(3)°, γ=102.82(3)°, Z=2,D c =1.785 g cm -3 ,μ=1.310mm -1 , R1=0.0184, wR2=0.0481, S=1.131.
[0031] [Cd(1,3-bdc)(3,3'-bpe)] n The single crystal structure diagram is shown in Figure 1 .
[0032] 2. [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)]n Synthesis
[0033] [Cd(1,3-bdc)(3,3'-bpe)] n (2.29 g, 5 mmol) was placed in a petri dish with a diameter of 15 cm and spread out. The petri dish was placed in the sun for exposure. After 2 hours, the sample was collected. Yield: 2.38 g, yield: 100%.
[0034] [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n Some crystallographic parameters: C 20 H 16 CdN2O5,M r =476.75,Triclinic, α=64.85(3)°, β=87.73(3)°, γ=75.14(3)°, Z=2,D c =1.750 g·cm -3 ,μ=1.242mm -1 , R1=0.0254, wR2=0.0713, S=1.119.
[0035] [Cd2(1,3-bdc)2(3,3'-tpcb)(H2O)2] n The single crystal structure diagram is shown in Figure 2 .
[0036] 3. [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n Synthesis
[0037] [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n (2.38 g, 5 mmol) was placed in an open reaction bottle, and the reaction bottle was placed in a vacuum drying oven at 120°C. After 1 hour, the reaction bottle was taken out of the drying oven and immediately sealed, and cooled to room temperature to obtain [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n . Yield: 2.29 g, yield: 100%.
[0038] [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n Some crystallographic parameters: C 20 H 14 CdN2O4,M r=458.74,Triclinic, α=112.88(3)°, β=90.29(3)°, γ=103.76(3)°, Z=2,D c =1.741 g·cm -3 ,μ=1.277mm -1 , R1=0.0211, wR2=0.0533, S=1.183.
[0039] 4. [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n Study on the air water extraction properties
[0040] 10g of coordination polymer material [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n Placed in a constant temperature and humidity chamber with a humidity of 20% and a temperature of 25°C, the material was weighed every 1 minute. After 10 minutes, the material's mass no longer increased. The weighing results showed that 10g of the coordination polymer increased its mass by 0.4g after absorbing water, and the amount of water absorbed was about 4% of its own weight. X-ray single crystal diffraction confirmed that the material absorbed moisture from low-humidity air to generate [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n .
Claims
1. A coordination polymer material, characterized in that: The coordination polymer material is [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n , wherein 3,3'-tpcb is 1,2,3,4-tetra(3-pyridyl)cyclobutane, 1,3-bdc is 1,3-phthalate, and n is the number of repeating units, which is any positive integer; The coordination polymer material is a crystalline inorganic-organic hybrid material, belonging to the triclinic system, Pī space group, and the unit cell parameters are α=112.88(3)°, β=90.29(3)°, γ=103.76(3)°.
2. A method for preparing the coordination polymer material according to claim 1, characterized in that The steps include: Step 1: Place 1,2-di(3-pyridyl)ethylene, 1,3-phthalic acid, cadmium nitrate tetrahydrate and deionized water in a polytetrafluoroethylene reactor, seal the reactor, and react under high temperature and high pressure. After the reaction is completed, slowly cool to room temperature to obtain colorless block crystals [Cd(1,3-bdc)(3,3'-bpe)] n , filter, wash, dry and collect block crystals; Step 2: The bulk crystals obtained in step 1 are placed under sunlight for photocatalytic cycloaddition reaction to generate [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n ; Step 3: Heat the colorless block crystals obtained in step 2 to 120°C to remove the water molecules in the pores to obtain the coordination polymer material [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n ; In step 1, bulk crystals [Cd(1,3-bdc)(3,3'-bpe)] n The unit cell parameters are: α=114.07(3)°, β=91.09(3)°, γ=102.82(3)°; In step 2, [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n The unit cell parameters are: α=64.85(3)°, β=87.73(3)°, γ=75.14(3)°.
3. An application of the coordination polymer material according to claim 1, characterized in that: The coordination polymer is used as an adsorption material in an air water extraction device to adsorb water vapor from the air and collect liquid water.
4. The use according to claim 3, characterized in that: The coordination polymer material [Cd(1,3-bdc)(3,3'-tpcb) 0.5 ] n When placed in a low humidity environment with an air humidity of 20%-30% for 10 minutes, it can absorb moisture in the environment and generate [Cd(1,3-bdc)(3,3'-tpcb) 0.5 (H2O)] n ; Through heating by solar collectors, the water adsorbed by the coordination polymer evaporates and condenses into liquid water, thereby realizing air circulation water extraction.