Emulsified asphalt and preparation method thereof
By using specific emulsifiers and composite stabilizers, the original asphalt is evenly dispersed in the aqueous phase, and the heat resistance and rut resistance of asphalt are improved through complexing and cross-linking techniques, the volatility and resistance of harmful gases under exposure to the sun are solved. The problem of insufficient rut capability has achieved a more durable asphalt pavement.
Patent Information
- Application Number
- CN202310177957.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-02-28
AI Technical Summary
Existing emulsified asphalt will evaporate harmful gases under the sun, which will damage human health. It has weak resistance to ruts after construction, which will easily soften and deform, resulting in undustable road surfaces.
Use polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and/or polyethylene glycol mono-4-tert-octylphenyl ether as emulsifiers, combining bismuth methylsulfonate, theophylline piperazine salt and ring mixing As a composite stabilizer, calcium acid is used to uniformly disperse the original asphalt in the water phase through complexing and crosslinking technology, improving the softening point and rut resistance, and adding plasticizer to form a spatial three-dimensional composite mesh structure to enhance the toughness of the asphalt and Resist stress.
It significantly improves the heat resistance and rut resistance of emulsified asphalt, reduces the volatility of harmful gases, extends the service life of asphalt pavement, and improves the crack and compressive resistance of the pavement, ensuring the stability and environmental protection of the pavement after construction. sex.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of paving materials, and more specifically, to an emulsified asphalt and a preparation method thereof. Background Art
[0002] Asphalt is a dark brown complex mixture of hydrocarbons of different molecular weights and their non-metallic derivatives. It is a high-viscosity organic liquid. Asphalt can be mainly divided into three types: coal tar asphalt, petroleum asphalt and natural asphalt. Among them, coal tar asphalt is a by-product of coking. Petroleum asphalt is the residue after crude oil distillation. Natural asphalt is stored underground, some of which form mineral layers or accumulate on the surface of the earth's crust. Asphalt is mainly used in industries such as coatings, plastics, rubber, and paving roads.
[0003] Emulsified asphalt refers to asphalt that is melted at low temperature and dispersed in an aqueous solution containing emulsifiers and their additives in the form of fine particles under mechanical stirring to form an oil-in-water (O / W) or water-in-oil (W / O) emulsion. Depending on the electrical properties of the emulsifier used, it is divided into cationic emulsified asphalt, anionic emulsified asphalt, non-ionic emulsified asphalt, etc.
[0004] Compared with high-temperature (170~200℃) hot asphalt, emulsified asphalt saves 40%~50% energy, improves construction conditions, reduces project costs by more than 20%~30%, and can effectively reduce excessive aging of asphalt caused by high-temperature heating and the large-scale volatilization of the carcinogen benzopyrene.
[0005] Emulsified asphalt has very low viscosity and good fluidity at room temperature. It can be used at room temperature and can be used with cold and wet stones. Emulsified asphalt is mainly used for road upgrading and maintenance, such as stone chip seal, and has many unique applications that cannot be replaced by other asphalt materials, such as cold mix and dilution slurry. Emulsified asphalt can also be used in new road construction, such as tack coat oil and penetration oil.
[0006] With the sharp increase in traffic volume and driving frequency, the axle weight of trucks is increasing. Now roads widely use one-way driving in different lanes, which requires further improvement of the road surface's anti-fluidity, that is, the ability to resist rutting at high temperatures, and improve flexibility and elasticity, that is, low-temperature crack resistance, wear resistance, and extended service life. After construction, general emulsified asphalt will still volatilize more harmful gases such as anthracene, phenanthrene, naphthalene, pyridine, etc. under the sun's exposure, which will damage human health. On the other hand, it is easy to soften, has weak anti-rutting ability, and the road surface is easy to deform. Summary of the invention
[0007] In order to improve the problem that general emulsified asphalt will still volatilize more harmful gases such as anthracene, phenanthrene, naphthalene, pyridine, etc. after construction and under the exposure to the sun, which is harmful to human health, and it is also easy to soften, has weak rutting resistance, and the road surface is easy to deform, the application proposes an emulsified asphalt and a preparation method thereof.
[0008] In a first aspect, the present application proposes an emulsified asphalt and adopts the following technical solution.
[0009] An emulsified asphalt, comprising the following raw materials in parts by weight:
[0010] 200-250 parts of original asphalt, 15-25 parts of emulsifier, 23-35 parts of composite stabilizer and water;
[0011] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and / or polyethylene glycol mono-4-tert-octylphenyl ether.
[0012] By adopting the above technical scheme, polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and / or polyethylene glycol mono-4-tert-octylphenyl ether contain rich hydrophilic groups and lipophilic groups, which can combine with the original asphalt and the water phase, so that the fine particles of the original asphalt are fully emulsified and dispersed in the water phase. The composite stabilizer can improve the dispersibility of the emulsifier, reduce the risk of emulsifier aggregation, and adjust the tension difference between the water phase and the oil phase, thereby improving the compatibility between the water phase and the oil phase. Polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and / or polyethylene glycol mono-4-tert-octylphenyl ether can complex anthracene, phenanthrene, naphthalene, pyridine and other components, making them difficult to dissociate, so that the softening point of the emulsified asphalt is significantly improved after construction and drying, that is, the heat resistance is improved, the anti-rutting ability is improved, and the asphalt pavement is not easy to deform.
[0013] As an improvement of the emulsified asphalt of the present application, the emulsifier is prepared by mixing polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and polyethylene glycol mono-4-tert-octylphenyl ether in a mass ratio of 10:(5-15).
[0014] By adopting the above technical solution, the emulsifier has stronger complexing and cross-linking capabilities, and has stronger binding ability with the original asphalt components. The structure after combination is stable and the softening point of the asphalt is significantly improved.
[0015] As an improvement of the emulsified asphalt of the present application, the composite stabilizer includes bismuth methanesulfonate, theophylline piperazine acetate and prohexadione calcium.
[0016] By adopting the above technical scheme, bismuth methanesulfonate, theophylline piperazine acetate and calcium cyclohexane improve the density of the water phase. The composite stabilizer also complexes with the emulsifier to improve the compatibility of the water phase and the oil phase, thereby stabilizing the emulsified asphalt components, improving the softening point and ductility, improving the toughness of the asphalt, and improving asphalt pavement cracks.
[0017] As an improvement of the emulsified asphalt of the present application, the composite stabilizer is prepared by mixing the bismuth methanesulfonate, the theophylline piperazine acetate and the calcium prohexadione in a mass ratio of (10-15): (10-15): (3-5).
[0018] By adopting the above technical solution, the composite stabilizer has a more significant stabilizing effect on the water phase and the oil phase.
[0019] As an improvement of the emulsified asphalt of the present application, the emulsified asphalt includes the following raw materials in parts by mass: 225 parts of original asphalt, 10 parts of polyoxyethylene alkylphenyl ether phosphate triethanolamine salt, 10 parts of polyethylene glycol mono-4-tert-octylphenyl ether, 12 parts of bismuth methanesulfonate, 12 parts of theophylline piperazine acetate, 4 parts of calcium cyclohexadione and water.
[0020] By adopting the above technical scheme, the original asphalt of the emulsified asphalt is complexed with polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and polyethylene glycol mono-4-tert-octylphenyl ether and evenly dispersed in the water phase. Bismuth methanesulfonate, theophylline piperazine acetate and calcium cyclohexadione reconcile the differences in density, tension and the like between the water phase and the oil phase, so that the water phase and the oil phase are mixed more evenly, so that the various components of the original asphalt are stably dispersed in the liquid. During construction, the coating is uniform, the structure is stable, it is resistant to high temperatures and it is not easy to volatilize harmful gases.
[0021] As an improvement of the emulsified asphalt of the present application, the emulsified asphalt further includes plasticizers bis(3,3,5-trimethylcyclohexyl) phthalate and / or cis-3,5,5-trimethylhexyl acetate.
[0022] By adopting the above technical scheme, bis(3,3,5-trimethylcyclohexyl) phthalate and / or cis-3,5,5-trimethylhexyl acetate can be complexed with the network structure composed of original asphalt, emulsifier, and composite stabilizer, bridge each layer of the network structure, and form a spatial three-dimensional composite network structure, thereby improving the structural strength of asphalt and improving toughness and pressure resistance.
[0023] As an improvement of the emulsified asphalt of the present application, the plasticizer is mixed by the following raw materials in parts by mass: 5 to 10 parts of bis(3,3,5-trimethylcyclohexyl) phthalate and 5 to 10 parts of cis-3,5,5-trimethylhexyl acetate.
[0024] By adopting the above technical solution, the spatial three-dimensional composite network structure formed has higher strength and stronger toughness.
[0025] As an improvement of the emulsified asphalt of the present application, the original asphalt is selected from a mixture of one or more of coal tar asphalt, petroleum asphalt and natural asphalt.
[0026] By adopting the above technical solution, there are multiple options for raw asphalt, which facilitates construction.
[0027] As an improvement of the emulsified asphalt of the present application, the emulsified asphalt includes 150 to 200 parts by mass of water.
[0028] By adopting the above technical solution, the water phase and the oil phase are evenly dispersed with each other, and the formed emulsion is more stable.
[0029] On the second aspect, the present application also proposes a method for preparing emulsified asphalt, and adopts the following technical solution.
[0030] A method for preparing emulsified asphalt, the preparation method comprising:
[0031] The raw asphalt, the emulsifier, the composite stabilizer and water are mixed, heated to 60-95° C., ground and sheared to uniformly disperse the raw asphalt into fine particles to form the oil-in-water type emulsified asphalt.
[0032] By adopting the above technical solution, the original asphalt is evenly dispersed at a relatively low temperature of 60-95°C, and an emulsified asphalt is prepared. The emulsified asphalt can be constructed at room temperature or heated to 60-95°C for better construction effect. Compared with the construction that requires a temperature of 170-200°C to melt the asphalt, which will volatilize a large amount of harmful gases, and the asphalt after such construction is easily softened under the sun, has weak anti-rutting ability, and is easy to deform the road surface, the solution of this application is more environmentally friendly, and the road surface after construction is also more solid, tough and not easy to deform.
[0033] In summary, the emulsified asphalt and the preparation method thereof of the present application have the following beneficial effects:
[0034] Polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and / or polyethylene glycol mono-4-tert-octylphenyl ether contain abundant hydrophilic and lipophilic groups, which can combine with the original asphalt and the water phase, fully emulsify the fine particles of the original asphalt and disperse them in the water phase. The composite stabilizer can improve the dispersibility of the emulsifier, reduce the risk of emulsifier aggregation, and adjust the tension difference between the water phase and the oil phase, thereby improving the compatibility of the water phase and the oil phase.
[0035] Polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and / or polyethylene glycol mono-4-tert-octylphenyl ether can complex anthracene, phenanthrene, naphthalene, pyridine and other components, making them difficult to dissociate, so that the softening point of the emulsified asphalt is significantly improved after construction and drying, that is, the heat resistance and anti-rutting ability are improved, making the asphalt pavement less likely to deform.
[0036] Plasticizers bis(3,3,5-trimethylcyclohexyl) phthalate and / or cis-3,5,5-trimethylhexyl acetate can complex with the network structure composed of original asphalt, emulsifier, and composite stabilizer, bridge each layer of the network structure, form a spatial three-dimensional composite network structure, enhance the structural strength of asphalt, and improve toughness and pressure resistance. DETAILED DESCRIPTION
[0037] The following is a detailed description of some embodiments, comparative examples and test examples of the emulsified asphalt and the preparation method thereof of the present application. Example 1
[0038] 200 g of original asphalt, 25 g of emulsifier, 23 g of composite stabilizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0039] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt.
[0040] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium. Example 2
[0041] The difference between this embodiment and embodiment 1 is that the ratio of each raw material is different.
[0042] Mix 250 g of original asphalt, 15 g of emulsifier, 35 g of composite stabilizer and 150 g of water, heat to 95°C, grind and shear, so that the original asphalt is evenly dispersed into fine particles to form water-in-oil emulsified asphalt.
[0043] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt.
[0044] The composite stabilizer is prepared by mixing 15 g of bismuth methanesulfonate, 15 g of theophylline piperazine acetate and 5 g of prohexadione calcium. Example 3
[0045] The difference between this embodiment and embodiment 1 is that the emulsifiers are different.
[0046] 200 g of original asphalt, 25 g of emulsifier, 23 g of composite stabilizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0047] The emulsifier is polyethylene glycol mono-4-tert-octylphenyl ether.
[0048] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium. Example 4
[0049] The difference between this embodiment and embodiment 2 is that the emulsifiers are different.
[0050] Mix 250 g of original asphalt, 15 g of emulsifier, 35 g of composite stabilizer and 150 g of water, heat to 95°C, grind and shear, so that the original asphalt is evenly dispersed into fine particles to form water-in-oil emulsified asphalt.
[0051] The emulsifier is polyethylene glycol mono-4-tert-octylphenyl ether.
[0052] The composite stabilizer is prepared by mixing 15 g of bismuth methanesulfonate, 15 g of theophylline piperazine acetate and 5 g of prohexadione calcium. Example 5
[0053] The difference between this embodiment and embodiment 1 is that the emulsifier includes two components.
[0054] 200 g of original asphalt, 15 g of emulsifier, 23 g of composite stabilizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0055] The emulsifier includes 10 g of polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and 5 g of polyethylene glycol mono-4-tert-octylphenyl ether.
[0056] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium. Example 6
[0057] The difference between this embodiment and embodiment 5 is that the ratio of the emulsifier is different.
[0058] 200 g of original asphalt, 25 g of emulsifier, 23 g of composite stabilizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0059] The emulsifier includes 10 g of polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and 15 g of polyethylene glycol mono-4-tert-octylphenyl ether.
[0060] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium. Example 7
[0061] The difference between this embodiment and embodiment 5 is that the proportions of the components are different and the emulsification temperatures are different.
[0062] 225 g of original asphalt, 20 g of emulsifier, 28 g of composite stabilizer and 200 g of water were mixed, heated to 80°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0063] The emulsifier includes 10 g of polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and 10 g of polyethylene glycol mono-4-tert-octylphenyl ether.
[0064] The composite stabilizer is prepared by mixing 12 g of bismuth methanesulfonate, 12 g of theophylline piperazine acetate and 4 g of prohexadione calcium. Example 8
[0065] The difference between this embodiment and embodiment 1 is that a plasticizer is further added in this embodiment.
[0066] 200 g of original asphalt, 25 g of emulsifier, 23 g of composite stabilizer, 10 g of plasticizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0067] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt.
[0068] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium.
[0069] The plasticizer is bis(3,3,5-trimethylcyclohexyl)phthalate. Example 9
[0070] The difference between this embodiment and embodiment 8 is that the types of plasticizers are different.
[0071] 200 g of original asphalt, 25 g of emulsifier, 23 g of composite stabilizer, 10 g of plasticizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0072] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt.
[0073] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium.
[0074] The plasticizer is cis-3,5,5-trimethylhexyl acetate. Example 10
[0075] The difference between this embodiment and embodiment 8 is that the plasticizer added in this embodiment comprises two components.
[0076] 200 g of original asphalt, 25 g of emulsifier, 23 g of composite stabilizer, 15 g of plasticizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0077] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt.
[0078] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium.
[0079] The plasticizer includes 5 g of bis(3,3,5-trimethylcyclohexyl)phthalate and 10 g of cis-3,5,5-trimethylhexyl acetate. Embodiment 11
[0080] The difference between this embodiment and embodiment 10 is that the ratio of the plasticizer added in this embodiment is different.
[0081] 200 g of original asphalt, 25 g of emulsifier, 23 g of composite stabilizer, 15 g of plasticizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0082] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt.
[0083] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium.
[0084] The plasticizer includes 10 g of bis(3,3,5-trimethylcyclohexyl)phthalate and 5 g of cis-3,5,5-trimethylhexyl acetate. Example 12
[0085] The difference between this embodiment and embodiment 7 is that a plasticizer is added in this embodiment.
[0086] 225 g of original asphalt, 20 g of emulsifier, 28 g of composite stabilizer, 15 g of plasticizer and 200 g of water were mixed, heated to 80°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0087] The emulsifier includes 10 g of polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and 10 g of polyethylene glycol mono-4-tert-octylphenyl ether.
[0088] The composite stabilizer is prepared by mixing 12 g of bismuth methanesulfonate, 12 g of theophylline piperazine acetate and 4 g of prohexadione calcium.
[0089] The plasticizer included 7 g of bis(3,3,5-trimethylcyclohexyl)phthalate and 8 g of cis-3,5,5-trimethylhexyl acetate.
[0090] Comparative Example 1
[0091] Compared with Example 1, the emulsifier in this comparative example is replaced by dodecyl dimethyl tertiary amine, as follows.
[0092] 200 g of original asphalt, 25 g of emulsifier, 23 g of composite stabilizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0093] The emulsifier is dodecyl dimethyl tertiary amine.
[0094] The composite stabilizer is prepared by mixing 10 g of bismuth methanesulfonate, 10 g of theophylline piperazine acetate and 3 g of prohexadione calcium.
[0095] Comparative Example 2
[0096] Compared with Example 1, the composite stabilizer in this comparative example is replaced with methyl cellulose, as follows.
[0097] 200 g of original asphalt, 25 g of emulsifier, 23 g of stabilizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0098] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt.
[0099] The stabilizer is methylcellulose.
[0100] Comparative Example 3
[0101] Compared with Example 1, the ratio of each component in this comparative example was adjusted as follows.
[0102] 200 g of original asphalt, 5 g of emulsifier, 3 g of composite stabilizer and 200 g of water were mixed, heated to 60°C, ground and sheared to evenly disperse the original asphalt into fine particles to form an oil-in-water emulsified asphalt.
[0103] The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt.
[0104] The composite stabilizer is prepared by mixing 1 g of bismuth methanesulfonate, 1 g of theophylline piperazine acetate and 1 g of prohexadione calcium.
[0105] Comparative Example 4
[0106] Compared with Example 4, the ratio of each component in this comparative example was adjusted as follows.
[0107] Mix 250 g of original asphalt, 5 g of emulsifier, 5 g of composite stabilizer and 150 g of water, heat to 95°C, grind and shear, so that the original asphalt is evenly dispersed into fine particles to form water-in-oil emulsified asphalt.
[0108] The emulsifier is polyethylene glycol mono-4-tert-octylphenyl ether.
[0109] The composite stabilizer is prepared by mixing 2g of bismuth methanesulfonate, 2g of theophylline piperazine acetate and 1g of prohexadione calcium.
[0110] Test Example 1
[0111] The emulsified asphalt prepared in Examples 1-12 and Comparative Examples 1-4 were subjected to the test items shown in Table 1, mainly in accordance with the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering", and the odor was detected by nose smell comparison.
[0112] Table 1 Performance test of emulsified asphalt prepared in Examples 1-12 and Comparative Examples 1-4
[0113] 15℃ elongation / cm (JTGE20-2011) Softening point / ℃(JTGE20-2011) Needle penetration at 25℃ (0.1mm) (JTGE20-2011) Bake at 80℃ for 4h and check the smell Freeze-thaw splitting tensile strength ratio (%) (JTG E20-2011) Example 1 126.3 85.6 47.3 No obvious odor 86.6 Example 2 128.4 84.9 47.0 No obvious odor 86.9 Example 3 137.1 87.2 46.6 No obvious odor 87.2 Example 4 136.6 88.3 46.8 No obvious odor 87.5 Example 5 145.9 89.2 47.5 No obvious odor 88.0 Example 6 148.2 90.0 47.4 No obvious odor 88.3 Example 7 153.7 92.1 47.1 No obvious odor 89.7 Example 8 139.5 88.1 48.8 No obvious odor 88.1 Example 9 138.2 88.4 48.2 No obvious odor 88.4 Example 10 143.4 88.8 47.9 No obvious odor 88.9 Embodiment 11 145.7 88.5 47.7 No obvious odor 88.7 Example 12 154.3 92.3 48.3 No obvious odor 90.1 Comparative Example 1 112.3 73.4 51.2 Exudes a noticeable odor 67.8 Comparative Example 2 116.8 83.7 52.3 No obvious odor 78.5 Comparative Example 3 115.4 79.6 54.4 Slight odor 79.4 Comparative Example 4 118.1 80.5 55.6 Slight odor 80.2
[0114] From the test results in Table 1, it can be concluded that the emulsified asphalt prepared in Examples 1-12 has the following characteristics after drying: (1) good ductility, indicating that it has strong toughness and strong recovery ability after slight deformation; (2) a relatively high softening point, indicating that it has good heat resistance, is not easy to soften under the sun, and has strong anti-rutting ability; (3) a relatively low needle penetration, indicating that it has high compressive strength and is not easy to deform; (4) there is no obvious odor after high-temperature baking at 80°C for 4 hours, which is more environmentally friendly; (5) the freeze-thaw splitting tensile strength is relatively high, indicating that it has high anti-freeze cracking performance.
[0115] Compared with Examples 1 and 2, Examples 3 and 4 change the emulsifier from polyoxyethylene alkylphenyl ether phosphate triethanolamine salt to polyethylene glycol mono-4-tert-octylphenyl ether, and their ductility and softening point are improved to a certain extent, and the anti-freeze cracking performance is also improved to a certain extent.
[0116] Compared with Examples 1-4, Examples 5 and 6 use an emulsifier mixed with polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and polyethylene glycol mono-4-tert-octylphenyl ether, and the ductility, softening point and anti-freezing cracking performance are further improved.
[0117] Compared with Example 5, Example 7 adopts a more suitable ratio, and its ductility, softening point and anti-freeze cracking performance are further improved.
[0118] Compared with Example 1, different plasticizers, bis(3,3,5-trimethylcyclohexyl) phthalate or cis-3,5,5-trimethylhexyl acetate, were added to Examples 8 and 9, respectively. The ductility, softening point and anti-freeze cracking properties of the products were all improved compared with those of the product in Example 1.
[0119] Compared with Examples 8 and 9, Examples 10 and 11 use a plasticizer mixed with bis(3,3,5-trimethylcyclohexyl) phthalate and 10g of cis-3,5,5-trimethylhexyl acetate, and their ductility, softening point and frost crack resistance are all improved compared with the product of Example 1.
[0120] Compared with Example 7, Example 12 adopts a formula of mixing two emulsifiers and two plasticizers, and its ductility, softening point and anti-freeze cracking properties reach the best state among all the examples.
[0121] Compared with Example 1, in Comparative Example 1, the emulsifier is replaced by triethanolamine salt of polyoxyethylene alkylphenyl ether phosphate with dodecyl dimethyl tertiary amine. The ductility, softening point and anti-freeze cracking performance are all reduced, and an obvious odor is emitted after baking at 80°C for 4 hours, indicating that the complexing ability of dodecyl dimethyl tertiary amine for harmful components is weak.
[0122] In Comparative Example 2, compared with Example 1, the composite stabilizer is replaced by methylcellulose from the combination of bismuth methanesulfonate, theophylline piperazine acetate and calcium cyclohexadione. Its ductility, softening point and anti-freeze cracking performance are all reduced, and the higher needle penetration reflects the reduction in its compressive strength.
[0123] Compared with Example 1, Comparative Example 3 has a significant change in the ratio of each component, and its ductility, softening point and anti-freeze cracking performance are all reduced.
[0124] Compared with Example 4, Comparative Example 4 has a significant change in the ratio of each component, and its ductility, softening point and anti-freeze cracking performance are all reduced.
[0125] Based on the results of the above embodiments, comparative examples and test examples, it can be seen that the emulsified asphalt of the present application can make the original asphalt fully dispersed and stably exist in the oil phase and the water phase, the compatibility of the water phase and the oil phase is good, and the emulsifier used can also complex anthracene, phenanthrene, naphthalene, pyridine and other components, making it difficult to dissociate them, so that after the emulsified asphalt is constructed and dried, the softening point is significantly improved, that is, the heat resistance is improved, and the anti-rutting ability is improved, so that the asphalt pavement is not easy to deform, and it is not easy to volatilize harmful gases such as anthracene, phenanthrene, naphthalene, pyridine, etc., which is more environmentally friendly than general asphalt and has a wide range of applications.
[0126] The above is only a preferred embodiment of the present application, and the protection scope of the present application is not limited to the above embodiment. All technical solutions under the concept of the present application belong to the protection scope of the present application. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present application should also be regarded as falling within the protection scope of the present application.
Claims
1. An emulsified asphalt, characterized in that: The emulsified asphalt comprises the following raw materials in parts by weight: 200-250 parts of original asphalt, 15-25 parts of emulsifier, 23-35 parts of composite stabilizer and water; The emulsifier is polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and / or polyethylene glycol mono-4-tert-octylphenyl ether; The composite stabilizer is prepared by mixing bismuth methanesulfonate, theophylline piperazine acetate and prohexadione calcium in a mass ratio of (10-15): (10-15): (3-5); The emulsified asphalt includes 150 to 200 parts by mass of water.
2. The emulsified asphalt according to claim 1, characterized in that The emulsifier is prepared by mixing polyoxyethylene alkylphenyl ether phosphate triethanolamine salt and polyethylene glycol mono-4-tert-octylphenyl ether in a mass ratio of 10: (5-15).
3. The emulsified asphalt according to claim 1, characterized in that The emulsified asphalt comprises the following raw materials in parts by mass: 225 parts of original asphalt, 10 parts of polyoxyethylene alkylphenyl ether phosphate triethanolamine salt, 10 parts of polyethylene glycol mono-4-tert-octylphenyl ether, 12 parts of bismuth methanesulfonate, 12 parts of theophylline piperazine acetate, 4 parts of prohexadione calcium and water.
4. The emulsified asphalt according to claim 1, characterized in that The emulsified asphalt also includes plasticizers such as bis(3,3,5-trimethylcyclohexyl) phthalate and / or cis-3,5,5-trimethylhexyl acetate.
5. The emulsified asphalt according to claim 4, characterized in that The plasticizer is prepared by mixing the following raw materials in parts by weight: 5 to 10 parts of bis(3,3,5-trimethylcyclohexyl) phthalate and 5 to 10 parts of cis-3,5,5-trimethylhexyl acetate.
6. The emulsified asphalt according to claim 1, characterized in that The raw asphalt is selected from a mixture of one or more of coal tar asphalt, petroleum asphalt and natural asphalt.
7. A method for preparing emulsified asphalt according to any one of claims 1 to 6, characterized in that: The preparation method comprises: The raw asphalt, the emulsifier, the composite stabilizer and water are mixed, heated to 60-95° C., ground and sheared to uniformly disperse the raw asphalt into fine particles to form the oil-in-water type emulsified asphalt.