A method and device for reducing oxygen potential in remelting atmosphere and improving cleanliness of electroslag ingot
By lowering the temperature of the protective gas and using active element particles to absorb oxygen, the problem of the influence of oxygen potential in electroslag remelting in a fully enclosed protective atmosphere is solved, and the cleanliness of the electroslag ingot and the quality of the steel ingot are significantly improved.
Patent Information
- Application Number
- CN202310065855.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-06
AI Technical Summary
In the fully closed protective atmosphere electroslag remelting process, although the oxygen content in the steel ingot can be effectively reduced, the weak oxygen partial pressure in the furnace still affects the quality of the steel ingot. Especially when smelting high-purity steel or alloys, there is an oxygen potential. Affect the quality of electroslag steel.
By lowering the temperature of the protective gas below -30°C, the gaseous water is condensed into a solid state, removing the moisture, and placing active element particles in the sealed space to react with the oxygen in the furnace and absorb oxygen, thereby reducing the oxygen potential in the remelting atmosphere. , improve the cleanliness of electroslag ingots.
It effectively reduces the oxygen content in the electroslag ingot, reduces the burning loss of easily oxidized elements, improves the cleanliness of the electroslag ingot and the mechanical properties of the final product, and ensures the uniformity of the head and tail components of the steel ingot.
Smart Images

Figure CN116121547B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method and a device for reducing the oxygen potential in a remelting atmosphere and improving the cleanliness of an electroslag ingot. Background Art
[0002] The electroslag remelting furnace is a metallurgical equipment that uses the resistance heat generated by electric current passing through molten slag as a heat source for smelting. Its structure mainly includes a crystallizer, a column located on one side of the crystallizer, and a horizontal cantilever is arranged above the column. The electrode rod extending downward into the crystallizer is installed on the horizontal cantilever facing the crystallizer, and is used to produce high-quality steel. The rapid development of science and technology has put higher and higher requirements on the quality of steel. In order to achieve higher performance of steel, improving its cleanliness is one of the important measures. In this context, the protective atmosphere electroslag furnace was applied.
[0003] Ordinary electroslag remelting is usually carried out under the atmosphere. A large number of studies have shown that in the general electroslag furnace process for smelting under the atmosphere, due to the direct transfer of oxygen and water vapor in the atmosphere to the metal molten pool through the slag, the high-temperature oxidation of the electrode surface above the slag surface brings active oxides into the slag pool, increasing the oxygen potential in the slag, thereby increasing the O content in the electroslag steel and causing serious burnout of easily oxidized elements such as Ti, Al, Mg, B, and Zr in the consumable electrode. In addition to directly reacting with the cations of the metal elements, the intervention of oxygen is more caused by the thermal oxidation of the electrodes above the slag. In the past few decades, in order to reduce the oxygen potential of the slag, the method of adding deoxidizers to the slag pool was usually adopted, but this would cause changes in the slag composition, resulting in the content of easily oxidized elements in the head and tail of the remelted ingot being inconsistent with the consumable electrode. The electroslag remelting technology using fully enclosed and controlled atmosphere protection no longer requires deoxidation of the slag, which can solve this problem well.
[0004] The fully enclosed protective atmosphere electroslag furnace uses an airtight inert gas protective cover, which not only prevents the electroslag steel from hydrogenating during the remelting process, but also prevents the atmosphere from oxidizing the metal electrodes and slag pool, so that the hydrogen, oxygen and nitrogen in the electroslag steel are not higher than the original content in the electrode blank. The easily oxidizable elements are burned very little during the remelting process. For example, the burning loss of titanium is negligible, while the burning loss of titanium in ordinary electroslag furnaces can reach 30% to 50%. In addition, the uniformity of the chemical composition of the electroslag ingot at the head and tail is also much better than that of the electroslag ingot produced by ordinary electroslag furnaces. Including the remelting of aluminum and titanium steel, the chemical composition deviation of the electroslag ingot at the head and tail of aluminum and titanium is extremely small.
[0005] The fully enclosed protective atmosphere electroslag furnace mainly prevents the oxidation of active metal elements in the steel during the remelting process by introducing inert gas into the enclosed protective cover. Most of them use argon protection, while nitrogen protection can be used for remelting nitrogen-containing steel. In addition, dry air protection can also be used simply to control the hydrogen content in the electroslag steel.
[0006] Experimental studies have shown that the use of protective atmosphere electroslag remelting can significantly reduce the burnout of elements and reduce the oxygen content in the ingot. However, due to the structure of the electroslag furnace, air tightness and the purity of the inert gas used (sometimes it may contain mixed gases, such as H 2 O, O 2 ) and other problems. When smelting high-purity steel or alloy, the weak oxygen partial pressure in the furnace will still affect the quality of electroslag steel. Therefore, it is necessary to adopt some unique means to reduce or avoid this situation. Summary of the invention
[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method and device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot. The method and device can reduce the oxygen potential in the fully enclosed protective atmosphere electroslag remelting smelting environment and improve the cleanliness of the electroslag ingot. This method reduces the temperature of the protective gas to below -30°C during the protective atmosphere electroslag remelting process, causing the gaseous water in the protective gas to condense into a solid state, thereby removing the moisture therein. Particles of active elements are placed in the device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot, so that they react with the residual O in the furnace, thereby removing the O in the atmosphere of the furnace, reducing the burning loss of easily oxidized elements in the electroslag ingot, and improving the cleanliness of the electroslag ingot, which is beneficial to improving the quality of the electroslag ingot and improving the mechanical properties of the final product.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] A method of reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot of the present invention needs to meet the following points:
[0010] (1) Electroslag remelting under sealing;
[0011] (2) Remove oxygen and moisture from the protective gas;
[0012] (3) An absorbent material that can react with oxygen is placed in the sealed space.
[0013] The method for removing oxygen and moisture from the protective gas is to use a protective gas with a temperature less than or equal to -30°C; or to set an absorbent that can react with oxygen and water at the protective gas inlet.
[0014] The absorbent capable of reacting with oxygen and water arranged at the protective gas inlet and the absorbent capable of reacting with oxygen arranged in the sealed space may be the same or different.
[0015] The specific operation includes the following steps:
[0016] (1) pouring molten slag that has reached a predetermined temperature into a crystallizer; sealing the crystallizer and the upper consumable electrode;
[0017] (2) A protective gas that removes oxygen is introduced into the confined space, and a consumable electrode is inserted into the slag pool to perform arcing, slag melting and electroslag remelting. The molten metal pool formed by the melting of the consumable electrode is cooled and solidified into an electroslag ingot;
[0018] (3) The high-temperature flue gas generated during electroslag remelting absorbs oxygen in the high-temperature flue gas through an absorbent material that can react with oxygen and is set in a closed space, thereby reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot.
[0019] By adopting the method of reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot of the present invention, the oxygen content in the electroslag ingot is below 15 ppm.
[0020] The protective gas is preferably Ar gas or N 2 gas.
[0021] In the method of reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot, the arc initiation and slag removal are: using a consumable electrode to directly initiate arc initiation and slag removal, and melting the slag through the consumable electrode. The method uses steel scraps as the arc initiation material, and then lowers the consumable electrode to the bottom of the crystallizer to contact the steel scraps, so that an arc will be generated immediately after the high voltage is turned on to melt the slag. Since the electrode is close to the arc initiation material at the beginning and the current is large, a smaller current should be set to allow the consumable electrode to continue to rise, and a larger heat is required to melt the slag in the slag removal stage, so a larger voltage should be set. The above current and voltage are determined according to the material of the consumable electrode and the slag used.
[0022] In the method of reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot, the electroslag remelting is: the metal droplets formed by the melting of the consumable electrode sink to the bottom of the liquid slag pool and gradually accumulate to form a metal molten pool; under the cooling effect of the crystallizer, a solidified electroslag ingot is gradually formed; the metal properties after electroslag remelting are significantly improved. At the beginning of remelting, since the consumable electrode is relatively cool, the consumable electrode cannot be inserted too deep, otherwise the consumable electrode will solidify together with the slag pool and cannot continue to be flame-refined. Therefore, the consumable electrode should be heated at a lower voltage for a period of time. After a period of time, in order to speed up the melting rate of the consumable electrode, the melting power should be continuously increased. As the consumable electrode melts shorter, the short network changes, and the power should begin to decrease.
[0023] In the method for reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot, cooling water is circulated in the cooling water channel inside the crystallizer and in the cooling water channel inside the cooling bottom plate. The slag is first dried in advance in the resistance furnace to remove moisture.
[0024] In the method for reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot, the absorbent capable of reacting with oxygen in the absorber is in a granular form, which can increase the reaction area. The temperature of the high-temperature flue gas is generally between 300 and 500°C. In this temperature range, the high-temperature flue gas is 2 The gas reacts quickly with the absorbent that can react with oxygen, thereby achieving the purpose of removing oxygen.
[0025] The absorbent capable of reacting with oxygen can be selected from Cu powder, Cu particles, Al powder, Al particles, sponge titanium and other active ingredients according to the composition of the smelting metal.
[0026] The present invention also provides a device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot, comprising a crystallizer, a fume hood, a cooling bottom plate, a refrigerator and an absorption device;
[0027] A smoke hood is arranged on the upper part of the crystallizer, and the smoke hood forms a closed space above the crystallizer, and an absorption device is arranged in the closed space; a cooling bottom plate is arranged below the crystallizer, and an air inlet is arranged on the smoke hood, and the refrigerator and / or the absorption device are connected to the air inlet of the smoke hood.
[0028] The device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot also includes a power supply and a consumable electrode; the consumable electrode extends into the interior of the crystallizer after passing through a closed space, one electrode of the power supply is connected to the consumable electrode, and the other electrode is connected to the cooling bottom plate; the power supply, power switch, consumable electrode, slag pool, metal molten pool, and cooling bottom plate form a power supply circuit; the thermal effect of the slag pool provides heat.
[0029] The crystallizer comprises a crystallizer body, in which a cooling water channel is arranged, and a water inlet and a water outlet are arranged.
[0030] The crystallizer body is preferably a cylindrical crystallizer body.
[0031] Furthermore, the smoke hood is divided into an upper smoke hood and a lower smoke hood. The upper smoke hood is used for convenient opening and sealing, and the lower smoke hood is used for setting multiple functional inlets and outlets.
[0032] The lower smoke hood is provided with an air inlet, a smoke exhaust port and a feeding port, and the feeding port of the lower smoke hood is connected with a feeding device.
[0033] The cooling bottom plate is provided with a cooling water channel, and is provided with a cooling bottom plate water inlet and a cooling bottom plate water outlet.
[0034] Preferably, the absorption device is arranged at the air inlet of the lower smoke hood.
[0035] The absorption device includes an absorption shell, which forms a cavity, and an absorption material that can react with oxygen is arranged in the cavity; holes are arranged on the absorption shell, and the diameter of the absorption material that can react with oxygen is greater than the diameter of the holes; through the absorption device, the high-temperature flue gas formed during the electroslag remelting process and the absorption device can function, thereby ensuring that the oxygen potential in the protective gas electroslag furnace system gradually decreases.
[0036] The refrigerator is used to reduce the temperature of the protective gas to below -30°C, thereby separating the gas and H 2 O separation.
[0037] The protective gas passes through the refrigerator, the smoke hood air inlet, and the absorption device to ensure the normal reaction in the electroslag furnace.
[0038] The present invention discloses a method and device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot. By absorbing and treating the protective gas, the smelting atmosphere in the crystallizer is deeply purified. Especially for the remelting of metals containing easily oxidizable elements, it is not only beneficial to reduce element burnout and facilitate the uniform control of the head and tail components of the electroslag ingot, but also beneficial to control the content of gases such as O and H in the electroslag ingot, reduce the content of oxide inclusions, and improve the cleanliness. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a schematic cross-sectional structure diagram of a device for reducing the oxygen potential in a remelting atmosphere and improving the cleanliness of an electroslag ingot according to Example 1 of the present invention;
[0040] Figure 2 This is a schematic cross-sectional structure diagram of a device for reducing the oxygen potential in a remelting atmosphere and improving the cleanliness of an electroslag ingot according to Example 2 of the present invention;
[0041] Figure 3 Three views of the absorption device; (a) is a front view, (b) is a side view, and (c) is a top view;
[0042] In the above figure, 1-power supply; 2-power switch; 3-consumable electrode; 4-upper smoke hood, 5-absorption device; 6-feeding device; 7-smoke exhaust port; 8-lower smoke hood air inlet; 9-cooler; 10-lower smoke hood; 11-slag pool; 12-crystallizer water outlet; 13-crystallizer body; 14-metal molten pool; 15-crystallizer water inlet; 16-cooling bottom plate body; 17-cooling bottom plate water outlet; 18-cooling bottom plate water inlet. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with embodiments.
[0044] In the embodiment of the present invention, the axes of the consumable electrode and the crystallizer coincide with each other.
[0045] In the embodiment of the present invention, the consumable electrode is connected to the dummy electrode, and the dummy electrode is suspended on the support arm of the electroslag furnace.
[0046] In the embodiment of the present invention, Cu chips are placed in the absorption device, which can increase the contact area between the active material and the furnace gas.
[0047] The diameter of the crystallizer in the embodiment of the present invention is 350 mm.
[0048] The diameter of the consumable electrode in the embodiment of the present invention is 250 mm.
[0049] The slag of the embodiment of the present invention contains the following components by mass percentage: CaF 2 50~70%, CaO 10~25%, Al 2 O 3 20~30%, MgO 0~5%.
[0050] The melting rate of the consumable electrode in the embodiment of the present invention is 200-400 kg / h.
[0051] The material of the consumable electrode in the embodiment of the present invention is G 20 Cr 2 Ni 4 A.
[0052] Example 1
[0053] A device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot in this embodiment is shown in the schematic diagram of the structure. Figure 1 , including a crystallizer body 13, an upper smoke hood 4, a lower smoke hood 10, a cooling bottom plate body 16, a refrigerator 9, an absorption device 5, a power supply 1, and a consumable electrode 3;
[0054] A lower smoke hood 10 is connected to the upper part of the crystallizer body 13, and an upper smoke hood 4 is connected above the lower smoke hood 10. The upper smoke hood 4 and the lower smoke hood 10 form a closed space above the crystallizer body 13, and an absorption device 5 is arranged on the side wall of the lower smoke hood; a cooling bottom plate body 16 is arranged below the crystallizer body 13, and the cooling bottom plate body 16 is provided with a cooling water channel, a cooling bottom plate water inlet 18 and a cooling bottom plate water outlet 17. A lower smoke hood air inlet 8 is arranged on the lower smoke hood 10, and a refrigerator 9 is connected to the lower smoke hood air inlet 8 through a pipeline.
[0055] The consumable electrode 3 extends to the inside of the crystallizer body 13 through the enclosed space, one electrode of the power supply 1 is connected to the consumable electrode 3, and the other electrode is connected to the cooling bottom plate body 16 through the power switch 2; the power supply 1, the power switch 2, the consumable electrode 3, the slag pool 11, the molten metal pool 14, and the cooling bottom plate body 16 form a power supply circuit; the thermal effect of the slag pool 11 provides heat.
[0056] A cooling water channel is arranged inside the crystallizer body 13 , and a crystallizer water inlet 15 and a crystallizer water outlet 12 are arranged.
[0057] In this embodiment, the crystallizer body 13 is a cylindrical crystallizer body. From top to bottom, the crystallizer includes a crystallizer water outlet 12, a cylindrical crystallizer body 13, and a crystallizer water inlet 15. A cooling water channel is provided in the crystallizer, and cooling water is introduced to provide cooling.
[0058] The lower smoke hood is also provided with a smoke exhaust port 7 and a feeding port, and the feeding port of the lower smoke hood is connected to the feeding device 6 .
[0059] The absorption device 5, its three-view drawing is shown in Figure 3 , including an absorption shell, the absorption shell forms a cavity, and copper particles are arranged in the cavity; holes are arranged on the absorption shell, and the diameter of the copper particles is greater than the diameter of the holes; through the absorption device, the high-temperature flue gas formed during the electroslag remelting process and the absorption device can function, thereby ensuring that the oxygen potential in the protective gas electroslag furnace system is gradually reduced.
[0060] The refrigerator is used to reduce the temperature of the protective gas to below -30°C, thereby separating the gas and H 2 O separation.
[0061] The protective gas passes through the refrigerator, the smoke hood air inlet, and the absorption device to ensure the normal reaction in the electroslag furnace.
[0062] The method of reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot in this embodiment adopts the above-mentioned device to improve the oxygen potential in the electroslag furnace, reduce the element burning loss, and improve the quality of the steel ingot. The specific method is:
[0063] Assemble the consumable electrode 3 onto the dummy electrode, and hang the dummy electrode on the crossbeam arm of the electroslag furnace, so that the axis of the consumable electrode 1 coincides with the axis of the crystallizer body 13;
[0064] Cooling water is introduced into the cooling water channel inside the crystallizer body 13, and cooling water is introduced into the cooling bottom plate body 16 arranged below the crystallizer;
[0065] Pour the preheated slag into the crystallizer body 13;
[0066] The lower smoke hood and the upper smoke hood are installed above the crystallizer body 13 to form a closed space, and the protective gas Ar gas is introduced into the closed space. Before the Ar gas is introduced, the temperature of the Ar gas is reduced to below 0°C by a cooler 9 to remove moisture in the protective gas, and then the Ar gas directly enters the closed space through the air pipe and the air inlet 8 of the lower smoke hood;
[0067] Use the consumable electrode to directly ignite the arc and melt the slag. Use steel scraps as the arc-ignition material, and then lower the consumable electrode to the bottom of the crystallizer to contact the steel scraps. In this way, an arc will be generated immediately after the high voltage is turned on to melt the slag.
[0068] After the high voltage is turned on, the metal droplets formed by the melting of the consumable electrode sink to the bottom of the liquid slag pool and gradually accumulate to form a molten metal pool; under the cooling effect of the crystallizer, a solidified electroslag ingot is gradually formed. During this process, the gas in the molten metal pool floats up and enters the slag pool, and finally enters the protective atmosphere. The gas temperature rises in the confined space, and the rising gas reacts with the Cu particles in the absorption device.
[0069] The melting rate of the consumable electrode is 200kg / h, the element burnout is small, the oxygen content in the electroslag ingot is reduced from 15-20ppm in the unpurified atmosphere in the smelting chamber to below 15ppm, and the ingot surface is smooth with excellent surface quality. The element burnout in the composition detection is less, which greatly improves the quality of the steel ingot.
[0070] Example 2
[0071] The schematic diagram of the structure of the device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot in this embodiment is shown in FIG. Figure 2 The specific structure is the same as that of Example 1; the difference is that the absorption device 5 is arranged at the air inlet 8 of the lower smoke hood.
[0072] The method is the same as in Example 1, except that:
[0073] The protective gas passes through the cooler 9 to reduce the temperature below -30°C, removes moisture from the protective gas, and directly enters the absorption device 5 through the lower smoke hood air inlet 8, reacts with copper scraps and copper particles, and then enters the electroslag furnace. At the same time, due to the reaction, the temperature continues to rise, and the gas rises to react with the copper scraps and copper particles in the absorption device. Further reduce the oxygen content. The oxygen content in the prepared electroslag ingot is reduced from 15-20ppm in the unpurified atmosphere of the smelting chamber to less than 10ppm, and the ingot surface is smooth and has excellent surface quality, which greatly improves the quality of the steel ingot.
[0074] Example 3
[0075] The device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot in this embodiment is the same as that in Embodiment 2, except that: no refrigerator is provided, and the oxygen content in the prepared electroslag ingot is reduced from 15-20ppm in the unpurified atmosphere in the smelting chamber to below 12ppm.
[0076] Comparative Example 1
[0077] A method for reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot only meets the requirement that the electroslag remelting is carried out under sealing, then the oxygen content in the closed space increases significantly, and the oxygen content in the electroslag ingot is 30-50ppm.
[0078] Comparative Example 2
[0079] A method for reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot only meets the following conditions: (1) electroslag remelting is performed under sealing; (2) a protective gas having a temperature of less than or equal to -30°C is introduced; then the oxygen content in the electroslag ingot is reduced to 15-20 ppm, indicating that no absorption device is provided and the protective gas contains only H 2 O separation, which also contains a small amount of impurity gases.
[0080] Comparative Example 3
[0081] A method for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot is the same as that of Example 1, except that: only (1) the electroslag remelting is performed under sealing; (3) an absorbing material capable of reacting with oxygen is arranged in the sealed space; the oxygen content in the electroslag ingot is reduced to 20-25 ppm, indicating that if the protective gas introduced into the sealed space is not subjected to low temperature treatment, the device is adopted. Compared with Example 1, no refrigerator is arranged, and the protective gas contains a small amount of H 2 O, so that the oxygen content in the electroslag ingot is slightly increased compared with Example 1.
Claims
1. A method for reducing the oxygen potential in a remelting atmosphere to improve the cleanliness of an electroslag ingot, characterized in that: Meet the following points: (1) Electroslag remelting under sealing; (2) Remove oxygen and moisture from the protective gas; (3) An absorbent material capable of reacting with oxygen is provided in the sealed space; The method for removing oxygen and moisture from the protective gas is to use a protective gas with a temperature of less than or equal to -30°C, or to provide an absorbent that can react with oxygen and moisture at the protective gas inlet; The method for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot comprises the following steps: Step 1. Pour the molten slag reaching a predetermined temperature into the crystallizer; seal the crystallizer and the upper consumable electrode; Step 2. A protective gas from which oxygen is removed is introduced into the confined space, and a consumable electrode is inserted into the slag pool to perform arcing, slag melting and electroslag remelting. The molten metal pool formed by the melting of the consumable electrode is cooled and solidified into an electroslag ingot; Step 3. The high-temperature flue gas generated during electroslag remelting is absorbed by an absorbent material capable of reacting with oxygen in a closed space, thereby reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot, so that the oxygen content in the electroslag ingot is below 15 ppm; In the method for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot, the arc initiation and slag melting are: using a consumable electrode to directly initiate arc initiation and slag melting, and melting the slag through the consumable electrode; using steel scraps as arc initiation materials, and then lowering the consumable electrode to the bottom of the crystallizer to contact the steel scraps, so that an arc will be generated immediately after the high voltage is turned on to melt the slag; because the electrode is close to the arc initiation material at the beginning and the current is large, a smaller current should be set to make the consumable electrode continue to rise, and a larger heat is required to melt the slag in the slag melting stage, so a larger voltage should be set.
2. The method for reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of electroslag ingots according to claim 1, characterized in that: In the method for reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of the electroslag ingot, the electroslag remelting is: the metal droplets formed by the melting of the consumable electrode sink to the bottom of the liquid slag pool and gradually accumulate to form a metal molten pool; under the cooling effect of the crystallizer, a solidified electroslag ingot is gradually formed; the metal properties after electroslag remelting are significantly improved; at the beginning of remelting, since the consumable electrode is relatively cool, the consumable electrode cannot be inserted too deep, otherwise the consumable electrode will solidify together with the slag pool and cannot continue to be flame-refined; therefore, the consumable electrode should be heated at a relatively low voltage for a period of time; after a period of time, in order to speed up the melting rate of the consumable electrode, the melting power should be continuously increased; as the consumable electrode melts and becomes shorter, the short network changes, and the power should begin to decrease.
3. The method for reducing the oxygen potential in the remelting atmosphere to improve the cleanliness of electroslag ingots according to claim 1, characterized in that: The absorbent capable of reacting with oxygen is determined according to the composition of the smelting metal and is selected from one or a mixture of Cu powder, Cu particles, Al powder, Al particles, and sponge titanium.
4. A device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of electroslag ingots, characterized in that: It includes a crystallizer, a fume hood, a cooling base, a freezer and an absorption device; A smoke hood is arranged on the upper part of the crystallizer, and the smoke hood forms a closed space above the crystallizer, and an absorption device is arranged in the closed space; a cooling bottom plate is arranged below the crystallizer, and an air inlet is arranged on the smoke hood, and the refrigerator and / or the absorption device are connected to the air inlet of the smoke hood.
5. The device for reducing oxygen potential in remelting atmosphere and improving cleanliness of electroslag ingot according to claim 4, characterized in that: The device for reducing the oxygen potential in the remelting atmosphere and improving the cleanliness of the electroslag ingot also includes a power supply and a consumable electrode; the consumable electrode extends into the interior of the crystallizer after passing through a closed space, one electrode of the power supply is connected to the consumable electrode, and the other electrode is connected to the cooling bottom plate; the power supply, power switch, consumable electrode, slag pool, metal molten pool, and cooling bottom plate form a power supply circuit; the thermal effect of the slag pool provides heat.
6. The device for reducing oxygen potential in remelting atmosphere and improving cleanliness of electroslag ingot according to claim 4, characterized in that: The crystallizer comprises a crystallizer body, in which a cooling water channel is arranged, and a water inlet and a water outlet are arranged; And / or, the smoke hood is divided into an upper smoke hood and a lower smoke hood; the lower smoke hood is provided with an air inlet, a smoke exhaust port, and a feed port, and the feed port of the lower smoke hood is connected to a feed device; And / or, the cooling bottom plate is provided with a cooling water channel, and is provided with a cooling bottom plate water inlet and a cooling bottom plate water outlet.
7. The device for reducing oxygen potential in remelting atmosphere and improving cleanliness of electroslag ingot according to claim 4, characterized in that: The absorption device includes an absorption shell, which forms a cavity, in which an absorption material capable of reacting with oxygen is arranged; holes are arranged on the absorption shell, and the diameter of the absorption material capable of reacting with oxygen is greater than the diameter of the holes; and when the absorption device is connected to the air inlet of the smoke hood, the absorption device is arranged at the lower smoke hood air inlet.