Waterborne coating composition for cans

By using a combination of acrylic modified epoxy resin, low melting point wax, polyolefin aqueous dispersion and phenolic resin in the water-based coating for tanks, the problem of difficulty in taking into account both slipability and wear resistance in the prior art is achieved. The coating film with excellent sliding, wear resistance and processability improves the overall performance of the can cover.

CN116135936BActive Publication Date: 2024-11-26KANSAI PAINT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211317520.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-18
Filing Date
2022-10-26
Publication Date
2024-11-26
Estimated Expiration
2042-10-26

Smart Images

  • Figure BDA0003909131940000171
    Figure BDA0003909131940000171
  • Figure BDA0003909131940000181
    Figure BDA0003909131940000181
  • Figure BDA0003909131940000191
    Figure BDA0003909131940000191
Patent Text Reader

Abstract

The present invention provides a water-based coating composition for cans having excellent sliding properties and wear resistance and excellent processability. The water-based coating composition for cans is characterized by comprising an acrylic modified epoxy resin (A), at least one wax (B) selected from the group consisting of three waxes having different melting points, an aqueous polyolefin dispersion (C) having an average particle size of 0.1 to 5 μm and a polyolefin penetration of 8 or less, and a phenolic resin (D) in a specific composition ratio.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] [CROSS-REFERENCE TO RELATED APPLICATIONS]

[0002] This application claims priority to invention patent application "Japanese Patent Application No. 2021-187496" filed with the Japan Patent Office on November 18, 2021, and all contents disclosed in that application are hereby incorporated as a whole into the description of this application. Technical Field

[0003] The present invention relates to a water-based coating composition for cans having excellent sliding properties, wear resistance and processability. Background Art

[0004] Metal cans are usually made of metal substrates such as aluminum, tin-free steel, and tinplate (galvanized iron). For the sake of formability, design, and metal surface protection, coatings are formed on the outer surfaces of cans, can lids, and pull rings obtained by processing these metal substrates. In particular, the coating of can lids is required to withstand the severe processing during molding, so internal wax-type can coatings containing wax in the coating have been developed to impart sliding properties.

[0005] For example, Patent Document 1 discloses a water-based coating composition for the outer surface of a can lid, which is a water-based coating composition for the outer surface of a can lid containing a pigment, a pigment dispersing resin and a binder resin, and is characterized in that the pigment dispersing resin is an acrylic copolymer having methacrylic acid, styrene and ethyl acrylate as constituent components.

[0006] In addition, Patent Document 2 discloses a water-based coating composition for the outer surface of a can, which contains a water-soluble acrylic resin (A) containing an animal wax (a) having a melting point of 40 to 70°C, an aqueous wax dispersion (B) containing the animal wax (a), a water-soluble polyester resin (C) and an amino resin (D).

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2006-176714

[0010] Patent Document 2: Japanese Patent Application Publication No. 2009-191180 Summary of the invention

[0011] Technical problem to be solved by the invention

[0012] However, in the coating compositions described in Patent Documents 1 and 2, if a large amount of wax is added to improve the sliding property of the coating film, the coating film becomes plasticized and the wear resistance decreases. Therefore, it is difficult to achieve both sliding property and wear resistance at a high level, and the processability may become insufficient.

[0013] The technical problem to be solved by the present invention is to provide a water-based coating composition for cans which has excellent sliding properties and wear resistance and also excellent processability.

[0014] Means used to solve problems

[0015] The present inventors have conducted intensive studies and have found that a coating composition comprising an acrylic modified epoxy resin, wax, a polyolefin aqueous dispersion and a phenolic resin can solve the above problems, thereby completing the present invention.

[0016] That is, the present invention relates to the following technical solutions:

[0017] 1. A water-based coating composition for cans, comprising an acrylic modified epoxy resin (A), a wax (B), a polyolefin aqueous dispersion (C) and a phenolic resin (D), characterized in that:

[0018] The wax (B) comprises at least one wax selected from the group consisting of a wax (b1) having a melting point lower than 50°C, a wax (b2) having a melting point of 50°C or higher and lower than 100°C, and a wax (b3) having a melting point of 100°C to 160°C and an average particle size of 1 μm to 15 μm,

[0019] The average particle size of the polyolefin aqueous dispersion (C) is 0.1 μm to 5 μm, and the needle penetration of the polyolefin is 8 or less.

[0020] Based on the total solid content of the acrylic modified epoxy resin (A), the total solid content of the wax (B) is 0.3% to 10% by mass, the total solid content of the polyolefin aqueous dispersion (C) is 1% to 10% by mass, and the total solid content of the phenolic resin (D) is 0.5% to 20% by mass.

[0021] 2. The aqueous can coating composition according to item 1 above, wherein the wax (b1) is at least one selected from the group consisting of lanolin wax, palm oil and triglyceride.

[0022] 3. The aqueous can coating composition according to item 1 or 2 above, wherein the wax (b2) is at least one selected from the group consisting of microcrystalline wax and carnauba wax.

[0023] 4. The aqueous coating composition for cans as described in any one of items 1 to 3 above, wherein the wax (b3) is at least one selected from the group consisting of polyethylene waxes and polypropylene waxes.

[0024] 5. The aqueous coating composition for cans as described in any one of items 1 to 4 above, wherein the solid content of the wax (b1), the wax (b2) and the wax (b3) is 0.1% by mass to 5% by mass of the wax (b1), 0.1% by mass to 5% by mass of the wax (b2), and 0.1% by mass to 5% by mass of the wax (b3), based on the total solid content of the acrylic modified epoxy resin (A).

[0025] 6. The aqueous coating composition for cans according to any one of claims 1 to 5, which is used for can lids.

[0026] 7. A can cap having a coating film of the aqueous coating composition for cans according to any one of 1 to 6 above.

[0027] Effects of the Invention

[0028] The aqueous coating composition for cans of the present invention can provide a coating film having excellent sliding properties and abrasion resistance and also excellent processability. DETAILED DESCRIPTION

[0029] The present invention relates to a water-based coating composition for cans (hereinafter sometimes referred to as the composition of the present invention), characterized by comprising an acrylic modified epoxy resin (A), a wax (B), a polyolefin aqueous dispersion (C) and a phenolic resin (D). Detailed description is given below.

[0030] <Water-based coating composition for cans>

[0031] <Acrylic modified epoxy resin (A)>

[0032] The acrylic modified epoxy resin (A) may be, for example, any of the following resins (1) and (2).

[0033] Resin (1): A resin obtained by subjecting a bisphenol epoxy resin (a1) (hereinafter sometimes referred to as “epoxy resin (a1)”) and a carboxyl group-containing acrylic resin (a2) (hereinafter sometimes referred to as “acrylic resin (a2)”) to an ester addition reaction.

[0034] The resin (1) can be obtained by, for example, heating the epoxy resin (a1) and the acrylic resin (a2) in an organic solvent in the presence of an esterification catalyst to facilitate an ester addition reaction.

[0035] Resin (2): A resin obtained by graft-polymerizing the epoxy resin (a1) with a polymerizable unsaturated monomer component containing a carboxyl group-containing polymerizable unsaturated monomer.

[0036] The resin (2) can be obtained by, for example, graft-polymerizing a polymerizable unsaturated monomer component and the epoxy resin (a1) in an organic solvent in the presence of a radical generator such as benzoyl peroxide.

[0037] The epoxy resin (a1) used in the above-mentioned resin (1) and the resin (2) may be, for example, any of the following: a resin obtained by polycondensing epichlorohydrin and bisphenol to a high molecular weight in the presence of a catalyst such as an alkali catalyst, a resin obtained by polyaddition reaction of a low molecular weight epoxy resin obtained by condensing epichlorohydrin and bisphenol in the presence of a catalyst such as an alkali catalyst, and a resin obtained by polyaddition reaction of the low molecular weight epoxy resin with bisphenol, and an epoxy ester resin obtained by reacting these resins or the above-mentioned low molecular weight epoxy resin with a dibasic acid.

[0038] Examples of the bisphenol include bis(4-hydroxyphenyl)methane [bisphenol F], 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane [bisphenol A], 2,2-bis(4-hydroxyphenyl)butane [bisphenol B], bis(4-hydroxyphenyl)-1,1-isobutane, bis(4-hydroxy-tert-butyl-phenyl)-2,2-propane, p-(4-hydroxyphenyl)phenol, oxybis(4-hydroxyphenyl), sulfonylbis(4-hydroxyphenyl), 4,4′-dihydroxybenzophenone, and bis(2-hydroxynaphthyl)methane. Among these, bisphenol A and bisphenol F are preferably used.

[0039] The above bisphenols may be used alone or in combination of two or more.

[0040] Examples of the dibasic acid used in the production of the epoxy ester resin include the following formula (1):

[0041] HOOC-(CH2) n -COOH...Formula (1)

[0042] (wherein n is an integer of 1 to 12), specifically, succinic acid, adipic acid, pimelic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexahydrophthalic acid, and the like can be exemplified.

[0043] Examples of commercially available epoxy resins (a1) include jER828 (epoxy equivalent of about 190), jER1007 (epoxy equivalent of about 1700), jER1009 (epoxy equivalent of about 3500), and jER1010 (epoxy equivalent of about 4500) manufactured by Mitsubishi Chemical Corporation, ARALDITE AER 6099 (epoxy equivalent of about 3500) manufactured by Asahi Ciba Co., Ltd., and EPOMIK R-309 (epoxy equivalent of about 3500) manufactured by Mitsui Chemicals, Inc.

[0044] As the epoxy resin (a1), from the viewpoint of corrosion resistance of the obtained coating film, a bisphenol type epoxy resin having a number average molecular weight of 2,000 to 35,000, preferably 4,000 to 30,000, and an epoxy equivalent of 1,000 to 12,000, preferably 3,000 to 10,000 can be preferably used.

[0045] In addition, the number average molecular weight in this specification is a value converted by using the molecular weight of standard polystyrene as a standard by the number average molecular weight measured by gel permeation chromatography (GPC).

[0046] Specifically, as the gel permeation chromatograph, "HLC 8120GPC" (trade name, manufactured by Tosoh Corporation) can be used, and as the chromatographic columns, four columns, namely "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL" and "TSKgel G-2000HXL" (trade names, all manufactured by Tosoh Corporation) can be used, and the measurement can be carried out under the conditions that the mobile phase is tetrahydrofuran, the measurement temperature is 40°C, the flow rate is 1 mL / min, and the detector is RI.

[0047] In the above-mentioned resin (1), during the ester addition reaction, the carboxyl group in the acrylic resin (a2) and the epoxy group in the epoxy resin (a1) undergo an ester addition reaction. Therefore, an epoxy group is required in the epoxy resin (a1), and the average number of epoxy groups per molecule of the epoxy resin is preferably 0.5 to 2, and particularly preferably in the range of 0.5 to 1.6.

[0048] On the other hand, in the resin (2), since the grafting reaction is initiated by hydrogen abstraction from the main chain of the epoxy resin and the graft polymerization reaction proceeds, the epoxy resin (a1) may not substantially contain epoxy groups.

[0049] The acrylic resin (a2) used in the above resin (1) is a copolymer resin containing a carboxyl group-containing polymerizable unsaturated monomer and other polymerizable unsaturated monomers as monomer components.

[0050] Examples of the carboxyl group-containing polymerizable unsaturated monomer include (meth)acrylic acid, maleic acid, crotonic acid, itaconic acid, fumaric acid and the like. These monomers may be used alone or in combination of two or more.

[0051] As for other polymerizable unsaturated monomers, any monomers that can be copolymerized with the above-mentioned carboxyl group-containing polymerizable unsaturated monomers can be appropriately selected and used according to the desired performance.

[0052] Specifically, there can be mentioned: aromatic vinyl monomers such as styrene, vinyl toluene, 2-methylstyrene, tert-butylstyrene, and chlorostyrene; acrylic acid or methacrylic acid having a carbon number of 2-ethylhexyl acrylate, n-octyl acrylate, decyl acrylate, lauryl acrylate, cyclohexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-, iso- or tert-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, octyl methacrylate, decyl methacrylate, lauryl methacrylate, cyclohexyl methacrylate, and the like. 1-18 carbon atom alkyl ester or cycloalkyl ester; 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate; 3-hydroxypropyl methacrylate, hydroxybutyl methacrylate and other hydroxyalkyl esters of acrylic acid or methacrylic acid with 2-8 carbon atoms; N-hydroxymethyl acrylamide, N-butoxymethyl acrylamide, N-methoxymethyl acrylamide, N-hydroxymethyl methacrylamide, N-butoxymethyl methacrylamide and other N-substituted acrylamide or N-substituted methacrylamide monomers, etc. The above other polymerizable unsaturated monomers can be used alone or in combination of two or more.

[0053] As the other polymerizable unsaturated monomer, a mixture of styrene and ethyl acrylate is particularly preferred, and the component composition mass ratio of styrene / ethyl acrylate is preferably in the range of 99.9 / 0.1 to 20 / 80, particularly preferably in the range of 99 / 1 to 40 / 60.

[0054] In the acrylic resin (a2), there are no particular restrictions on the types and constituent ratios of the monomers, but generally, the carboxyl-containing polymerizable unsaturated monomer is preferably 15 to 80% by mass, particularly preferably 20 to 60% by mass, and the other polymerizable unsaturated monomers are 85 to 20% by mass, particularly preferably 80 to 40% by mass.

[0055] The acrylic resin (a2) can be synthesized by polymerizing the above-mentioned monomer mixture in an organic solvent in the presence of a polymerization initiator to facilitate the reaction. The acrylic resin (a2) preferably has a resin acid value of 100 to 400 mgKOH / g and a number average molecular weight of 5,000 to 100,000.

[0056] The above reaction can be carried out by a known method, for example, by mixing an esterification catalyst in a uniform organic solvent solution of the epoxy resin (a1) and the acrylic resin (a2) and reacting them at a reaction temperature of 60 to 130° C. for about 1 to 6 hours until substantially all the epoxy groups are consumed. Examples of the above esterification catalyst include tertiary amines such as triethylamine and dimethylethanolamine, and quaternary salt compounds such as triphenylphosphine, among which tertiary amines are preferably used.

[0057] The solid content concentration in the reaction system of the epoxy resin (a1) and the acrylic resin (a2) is not particularly limited as long as the reaction system is within a viscosity range that does not affect the reaction. In addition, when an esterification catalyst is used in the ester addition reaction, its usage amount is usually preferably used in the range of 0.1 to 1 equivalent relative to 1 equivalent of epoxy groups in the epoxy resin (a1).

[0058] When the acrylic modified epoxy resin is the above-mentioned resin (2), the polymerizable unsaturated monomer component containing a carboxyl group-containing polymerizable unsaturated monomer to be graft-polymerized with the epoxy resin (a1) can include: a carboxyl group-containing polymerizable unsaturated monomer as a monomer component used in the preparation of the carboxyl group-containing acrylic resin (a2) in the above-mentioned resin (1) and other polymerizable unsaturated monomers.

[0059] The graft polymerization reaction in the resin (2) can be carried out by a known method, for example, by slowly adding a uniform mixed solution of a free radical generator and a polymerizable unsaturated monomer component to an organic solvent solution of the epoxy resin (a1) heated to 80 to 150° C., and maintaining the mixture at the same temperature for about 1 to 10 hours. Examples of the free radical generator include azobisisobutyronitrile, benzoyl peroxide, tert-butyl peroxybenzoyloctanoate, tert-butyl peroxy-2-ethylhexanoate, and the like.

[0060] As the organic solvent, any known organic solvent can be used, as long as it is an organic solvent that dissolves the epoxy resin (a1), the acrylic resin (a2) or the polymerizable unsaturated monomer component containing a carboxyl group and does not hinder the formation of an emulsion when the acrylic modified epoxy resin (A) which is the reaction product of these is neutralized and made aqueous.

[0061] Specific examples of the organic solvent include isopropyl alcohol, butanol, 2-hydroxy-4-methylpentane, 2-ethylhexanol, cyclohexanol, ethylene glycol, diethylene glycol, 1,3-butanediol, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, and diethylene glycol monomethyl ether.

[0062] The acrylic modified epoxy resin as the resin (1) or (2) has a carboxyl group, and from the viewpoint of dispersibility, coating performance, etc., the resin acid value is preferably in the range of 10 to 160 mgKOH / g, particularly preferably 20 to 100 mgKOH / g.

[0063] The acrylic modified epoxy resin can be dispersed in an aqueous medium by neutralizing at least a portion of the carboxyl groups in the resin with a basic compound.

[0064] As the alkaline compound, amines, ammonia, etc. can be preferably used. As the amine, specifically, alkylamines such as trimethylamine, triethylamine, and tributylamine, alkanolamines such as dimethylethanolamine, diethanolamine, and aminomethylpropanol, cyclic amines such as morpholine, etc. There is no particular limitation on the neutralization degree of the acrylic modified epoxy resin, but it is usually preferably in the range of 0.1 to 2.0 equivalents relative to the carboxyl group in the resin.

[0065] The aqueous medium may be water alone or a mixture of water and an organic solvent. As the organic solvent, a known organic solvent may be used, and preferably, those organic solvents listed as the organic solvents that can be used in the manufacture of the acrylic modified epoxy resin may be used. The amount of the organic solvent in the composition of the present invention is preferably 20% by mass or less, and particularly preferably 10% by mass or less, relative to the total amount of the resin solid content of the composition of the present invention from the viewpoint of environmental protection, etc.

[0066] The dispersion of the acrylic modified epoxy resin in the aqueous medium can be carried out by conventional methods, for example, a method in which the acrylic modified epoxy resin is slowly added under stirring to an aqueous medium containing an alkaline compound as a neutralizing agent; a method in which the acrylic modified epoxy resin is neutralized with an alkaline compound and then the aqueous medium is added to the neutralized product under stirring; or a method in which the neutralized product is added to an aqueous medium.

[0067] <Wax (B)>

[0068] Specific examples of the wax (B) include natural waxes, synthetic waxes, glycerides, waxes, and oxides and acid-modified products thereof, and these may be used alone or in combination of two or more.

[0069] As natural waxes, for example, hydrogenated solidified fats such as hydrogenated beef tallow or lard, beeswax, lanolin wax, spermaceti, hydrogenated spermaceti, carnauba wax, candelilla wax, rice wax, wood wax, jojoba wax, shellac and other animal and plant waxes, paraffin wax, microcrystalline wax, montan wax, ozokerite and other mineral waxes, etc.

[0070] Examples of the synthetic wax include polyethylene wax, polypropylene wax, polytetrafluoroethylene wax, and silicone wax.

[0071] As the wax (B), from the viewpoint of sliding property and abrasion resistance, lanolin wax, olive oil, palm oil, linseed oil, microcrystalline wax, polyethylene wax and the like can be preferably used.

[0072] Commercially available products of the wax (B) include purified lanolin (lanolin wax, trade name, manufactured by CRODA), CERACOL 609N (lanolin wax, trade name, manufactured by BYK), lanolin R (lanolin wax, trade name, manufactured by Nippon Seika Co., Ltd.), Outer Lo-1 (olive oil, trade name, manufactured by Riken Vitamin Co., Ltd.), refined palm oil (palm oil, trade name, manufactured by Nissin Oil Manufacturing Co., Ltd.), HI-DISPER 1260 (microcrystalline wax, trade name, manufactured by Gifu Shellac Manufacturing Co., Ltd.), TOPCO S923 (microcrystalline wax, trade name, manufactured by Toyo Petrolite Co., Ltd.), CERAFLOUR 991 (manufactured by BYK, trade name, polyethylene wax, average particle size 5 μm, melting point 115° C.), HIGH FLAT2352 (manufactured by Gifu Shellac Manufacturing Co., Ltd., trade name, oxidized polyethylene wax, average particle size 5 μm, melting point 138° C.), Lanco1370LF (manufactured by Lubrizol Corporation, trade name, polypropylene wax, average particle size 9 μm, melting point 150° C.), etc.

[0073] The amount of the wax (B) varies depending on the type of wax used, but from the viewpoint of sliding properties and wear resistance, it is preferably in the range of 0.3 to 10% by mass, more preferably 0.3 to 6% by mass, and even more preferably 0.5 to 1.5% by mass, based on the total solid content of the acrylic modified epoxy resin (A) (the total solid content of the acrylic modified epoxy resin (A) being 100% by mass).

[0074] The composition of the present invention uses at least one wax selected from the group consisting of a wax (b1) having a melting point less than 50°C, a wax (b2) having a melting point of 50°C or more and less than 100°C, and a wax (b3) having a melting point of 100-160°C and an average particle size of 1-15 μm from the above-mentioned wax (B).

[0075] By using at least one selected from the above three waxes, the surface roughness of the coating film can be adjusted, and a can body having a reduced dynamic friction coefficient, excellent sliding properties, wear resistance and processability, and excellent cover-forming properties can be provided.

[0076] Wax (b1)

[0077] The wax (b1) is not particularly limited as long as it has a melting point of less than 50°C. From the viewpoint of reducing the dynamic friction coefficient and improving sliding properties, wear resistance and processability, lanolin wax, olive oil, palm oil, linseed oil, triglycerides and the like are preferably used.

[0078] Commercially available products of the wax (b1) include purified lanolin (lanolin wax, trade name, manufactured by CRODA), Outer Lo-1 (olive oil, trade name, manufactured by Riken Vitamin Co., Ltd.), and purified palm oil (palm oil, trade name, manufactured by Nissin Oil Separation Co., Ltd.).

[0079] Wax (b2)

[0080] The wax (b2) is not particularly limited as long as it has a melting point of 50°C or higher and less than 100°C, preferably 60 to 90°C. From the viewpoint of reducing the dynamic friction coefficient and improving sliding properties, wear resistance and processability, microcrystalline wax and carnauba wax are preferably used.

[0081] In addition, commercially available products of the wax (b2) include HI-DISPER 1260 (microcrystalline wax, trade name, manufactured by Gifu Shellac Manufacturing Co., Ltd.), TOPCO S923 (microcrystalline wax, trade name, manufactured by Toyo Petrolite Co., Ltd.), HD-3028 (manufactured by Gifu Shellac Manufacturing Co., Ltd., carnauba wax, melting point 82°C), and Hi-Mic-1070 (manufactured by Nippon Seifuku Co., Ltd., microcrystalline wax, melting point 80°C).

[0082] Wax (b3)

[0083] The wax (b3) is not particularly limited as long as it has an average particle size of 1 to 15 μm, preferably 2 to 11 μm, and a melting point of 100 to 160°C, preferably 120 to 155°C. From the perspective of reducing the dynamic friction coefficient, improving sliding properties, wear resistance and processability, polyethylene wax and polypropylene wax can be preferably used.

[0084] In addition, commercially available products of the wax (b3) include, for example, CERAFLOUR 991 (manufactured by BYK, trade name, polyethylene wax, average particle size 5 μm, melting point 115°C), HIGH FLAT 2352 (manufactured by Gifu Shellac Manufacturing Co., Ltd., trade name, oxidized polyethylene wax, average particle size 5 μm, melting point 138°C), and Lanco 1370LF (manufactured by Lubrizol Corporation, trade name, polypropylene wax, average particle size 9 μm, melting point 150°C).

[0085] In the present invention, the melting point of the wax (B) refers to the endothermic peak temperature measured by a differential scanning calorimeter (DSC) at a heating rate of 10°C / min. In addition, when the wax has multiple endothermic peaks, the maximum endothermic peak is taken as the melting point. In addition, the average particle size of the wax is measured by a volume average particle size using Microtrac UPA (a particle size analyzer manufactured by Nikkiso Co., Ltd.) by a laser diffraction scattering method.

[0086] When the wax (B) includes the wax (b1), the solid content of the wax (b1) in the wax (B) is preferably in the range of 0.1 to 5% by mass, more preferably 0.2 to 2% by mass, and even more preferably 0.2 to 1.0% by mass, based on the total solid content of the acrylic modified epoxy resin (A), from the viewpoint of reducing the dynamic friction coefficient and improving the sliding property, wear resistance, and processability. When the wax (B) includes the wax (b2), the solid content of the wax (b2) in the wax (B) is preferably in the range of 0.1 to 5% by mass, preferably 0.2 to 2% by mass, and even more preferably 0.2 to 1.0% by mass, based on the total solid content of the acrylic modified epoxy resin (A), which is desirable from the viewpoint of reducing the dynamic friction coefficient, sliding property, wear resistance, and processability. When the wax (B) includes the wax (b3), from the viewpoint of reducing the dynamic friction coefficient, improving the sliding property, the wear resistance and the processability, the solid content of the wax (b3) in the wax (B) is preferably in the range of 0.1 to 5% by mass, more preferably 0.2 to 2% by mass, and further preferably 0.2 to 1.0% by mass, based on the total solid content of the acrylic modified epoxy resin (A). In addition, the total solid content of the wax (b1), the wax (b2) and the wax (b3) based on the total solid content (100% by mass) of the wax (B) can be, for example, 85% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, and further preferably 99% by mass or more.

[0087] <Polyolefin Aqueous Dispersion (C)>

[0088] The polyolefin aqueous dispersion (C) may be any one that can be dispersed in an aqueous composition such as an aqueous coating, an aqueous dispersion or an aqueous emulsion. A polyolefin aqueous dispersion obtained by emulsion polymerization, a polyolefin aqueous dispersion obtained by mechanically dispersing a polyolefin in an aqueous medium, etc. may be used. One type may be used alone or two or more types may be used in combination.

[0089] In the composition of the present invention, from the viewpoint of minimizing the use of an emulsifier and from the viewpoint of water resistance and the like, a polyolefin aqueous dispersion obtained by mechanically dispersing a polyolefin in an aqueous medium can be preferably used.

[0090] The polyolefin in the polyolefin aqueous dispersion (C) preferably has an average particle size of 0.1 to 5 μm, particularly preferably 0.2 to 4.0 μm, and even more preferably 0.3 to 3.0 μm, from the viewpoint of the sliding property, abrasion resistance, and processability of the resulting coating film.

[0091] In the composition of the present invention, the average particle size of the aqueous polyolefin dispersion (C) is a value measured by the Microtrac method.

[0092] In the composition of the present invention, the polyolefin in the polyolefin aqueous dispersion (C) preferably has a needle penetration of 8 or less, particularly preferably 4 or less, and even more preferably 1 or less, from the viewpoint of processability and abrasion resistance.

[0093] The penetration of the polyolefin constituting the polyolefin aqueous dispersion (C) is a value obtained by normalizing the penetration of a needle of a predetermined weight into the polyolefin at a temperature of 25° C., a load of 100 g, and a penetration time of 5 seconds according to JIS K 2207, and the penetration value is expressed as 1 penetration with 0.1 mm. Therefore, the smaller the penetration of the polyolefin, the harder it is, and the larger the penetration, the softer it is. The present invention uses an aqueous polyolefin dispersion obtained from a polyolefin having a penetration within the above range.

[0094] Examples of the types of polyolefin include low-density polyolefin, low-molecular-weight polyolefin, ethylene-methacrylic acid copolymer, and ionomers such as metal salts of ethylene-methacrylic acid copolymer.

[0095] Among the above, low molecular weight polyolefins, particularly low molecular weight polyethylene, can be preferably used from the viewpoint of water dispersibility.

[0096] As the polyolefin aqueous dispersion (C), commercial products may be used, and specific examples of commercial products include ARROWBASE manufactured by UNITIKA Co., Ltd., CHEMIPEARL manufactured by Mitsui Chemicals, Inc., and AB-50 manufactured by Gifu Shellac Manufacturing Co., Ltd.

[0097] The amount of the polyolefin aqueous dispersion (C) can be adjusted according to the desired degree of sliding, wear resistance and processability, and two or more kinds of polyolefins can be used in combination. From the viewpoint of sliding, wear resistance and processability, the total solid content of the polyolefin is preferably 1.0 to 10.0% by mass, particularly preferably 2.0 to 8.0% by mass, and more particularly preferably 3.0 to 7.0% by mass relative to the total solid content of the acrylic modified epoxy resin (A).

[0098] Phenolic resin (D)

[0099] Examples of the phenolic resin (D) include resol-type phenolic resins obtained by condensing a phenolic compound, a phenol (d1) such as bisphenol A, and an aldehyde (d2) such as formaldehyde in the presence of a reaction catalyst to introduce a methylol group.

[0100] Examples of the phenols (d1) include difunctional phenol compounds such as o-cresol, p-cresol, p-tert-butylphenol, p-ethylphenol, 2,3-xylenol, and 2,5-xylenol; trifunctional phenol compounds such as carbolic acid, m-cresol, m-ethylphenol, 3,5-xylenol, and m-methoxyphenol; and tetrafunctional phenol compounds such as bisphenol A and bisphenol F. One of the phenol compounds may be used alone or two or more thereof may be used in combination.

[0101] Examples of the aldehydes (d2) include formaldehyde, paraformaldehyde, trioxane, and the like, and these aldehydes may be used alone or in combination of two or more.

[0102] The methylol groups of the methylolated phenolic resin may be further alkyl-etherified. As the alcohol used in the alkyl-etherification, for example, monohydric alcohols having 1 to 6 carbon atoms, particularly preferably 1 to 4 carbon atoms, may be preferably used. Preferred monohydric alcohols include methanol, ethanol, n-propanol, n-butanol, isobutanol, and the like.

[0103] From the viewpoint of reactivity, the phenol resin (D) preferably has a number average molecular weight of 200 to 2000, particularly preferably 300 to 1200, and an average number of methylol groups per benzene nucleus of 0.3 to 3.0, particularly 0.5 to 3.0.

[0104] From the viewpoint of processability, the amount of the phenol resin (D) is preferably in the range of 0.5 to 20% by mass, particularly preferably 1 to 15% by mass, and even more preferably 2 to 10% by mass based on the total solid content of the acrylic modified epoxy resin (A).

[0105] <Water-based coating composition for cans>

[0106] The aqueous coating composition for cans of the present invention is an aqueous coating composition in which an acrylic modified epoxy resin (A) is neutralized and dispersed in an aqueous medium, and the composition contains wax (B), a polyolefin aqueous dispersion (C) and a phenolic resin (D) as essential components, and may optionally contain other additives such as surfactants, defoamers, pigments, fragrances, etc.

[0107] Among them, a surfactant can be preferably used from the viewpoint of dispersion stability of the polyolefin (component C) and stability of the coating film appearance when a pigment is contained.

[0108] As the surfactant, for example, alkylbenzenesulfonic acid (and amine-neutralized products) and the like can be particularly preferably used.

[0109] The solid content concentration of the composition of the present invention is not particularly limited, but is preferably in the range of 20 to 45% by mass, more preferably 22 to 40% by mass, from the viewpoint of coating stability.

[0110] The composition of the present invention can be used for various substrates, for example, the following substrates can be mentioned: metals such as tin-plated iron, aluminum, tin-free steel, iron, zinc, copper, galvanized steel sheets, alloy-plated steel sheets, etc., chemical conversion-treated metal sheets subjected to surface treatments such as phosphate treatment and chromate treatment on these metals, metal sheets coated with primers such as epoxy resins and vinyl resins on these metal sheets, and substrates obtained by processing these metal sheets into cans, etc.

[0111] The composition of the present invention can be preferably used for the inner and outer surfaces of cans, and particularly preferably used for can covers having strict requirements on cover-making properties.

[0112] The coating of the composition of the present invention is carried out by a known method, for example, by a coating method such as roller coating or spraying so that the dry film thickness becomes 1 to 20 μm, preferably 2 to 10 μm, and by a method of heat drying the raw material by maintaining it at a temperature of 120 to 300° C., preferably 200 to 280° C. for about 10 seconds to 30 minutes, preferably about 15 seconds to about 15 minutes.

[0113] Example

[0114] The present invention is described in more detail below by way of examples and comparative examples. The present invention is not limited by the following examples. In addition, the following "parts" and "%" are based on mass.

[0115] Production of acrylic acid modified epoxy resin (A)

[0116] Preparation Example 1 Preparation of Epoxy Resin No. 1 Solution

[0117] 558 parts of jER 828 (Note 1), 329 parts of bisphenol A and 0.6 parts of tetrabutylammonium bromide were placed in a glass four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet, and reacted at 160°C under a nitrogen stream. The reaction was followed by epoxy equivalent, and an epoxy resin No. 1 solution was obtained after about 5 hours of reaction. The number average molecular weight of the obtained epoxy resin No. 1 was about 8000.

[0118] (Note 1) jER828: manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, epoxy equivalent weight about 190, number average molecular weight about 380;

[0119] Preparation Example 2 Preparation of Epoxy Resin No. 2 Solution

[0120] 550 parts of jER828 (Note 1) and 450 parts of bisphenol A were added to a glass four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet, and the temperature was raised under a nitrogen stream while stirring. When bisphenol A was dissolved and the mixture became transparent (around 100°C), 5.0 parts of tri-n-butylamine was added, and the reaction was carried out at 160°C under a nitrogen stream.

[0121] The reaction was followed by epoxy equivalent, and the epoxy resin No. 2 solution was obtained after the reaction for about 4 hours. The number average molecular weight of the obtained epoxy resin No. 2 was about 4,500.

[0122] Preparation Example 3 Preparation of acrylic resin solution

[0123] 882 parts of n-butanol were added to a glass four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet, and a mixture of "180 parts of methacrylic acid, 240 parts of styrene, 180 parts of ethyl acrylate and 18 parts of tert-butyl peroxy-2-ethylhexanoate" was heated to 100°C under a nitrogen stream and added dropwise from a dropping funnel over about 3 hours, and after the addition, stirring was continued at the same temperature for 2 hours, followed by cooling to obtain an acrylic resin solution having a solid content of 40%. The obtained acrylic resin had a number average molecular weight of about 19,000 and an acid value of 196 mgKOH / g.

[0124] Preparation Example 4 Preparation of Acrylic Modified Epoxy Resin No. 1 Aqueous Dispersion

[0125] In a glass four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet, 80 parts (solid content) of the epoxy resin No. 1 solution obtained in Preparation Example 1, 20 parts (solid content) of the acrylic resin solution obtained in Preparation Example 3, and 33 parts of diethylene glycol monobutyl ether were added, heated to 100°C to dissolve, and then 2 parts of N,N-dimethylaminoethanol were added to react for about 2 hours, and then 3 parts of N,N-dimethylaminoethanol were added to continue the reaction for 20 minutes. Then, 165 parts of deionized water were added dropwise over 1 hour to obtain an acrylic modified epoxy resin No. 1 aqueous dispersion having an acid value of 34 mgKOH / g and a solid content of 30%.

[0126] Preparation Example 5 Preparation of Acrylic Modified Epoxy Resin No. 2 Aqueous Dispersion

[0127] In a glass four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet, 25 parts of ethylene glycol monobutyl ether and 80 parts (solid content) of the epoxy resin No. 2 solution obtained in Production Example 2 were added, and the temperature was raised to 120° C. under a nitrogen flow while stirring.

[0128] After the epoxy resin No. 2 solution was completely dissolved, a mixed solution of "4 parts of styrene, 4 parts of methyl methacrylate, 6 parts of n-butyl acrylate, 6 parts of methacrylic acid, and 1 part of benzoyl peroxide" was added dropwise at 120°C for 1 hour. After the addition was completed, the mixture was kept at 120°C for 1 hour. Then, the mixture was cooled to 90°C, 6.2 parts of dimethylethanolamine were added, and the mixture was stirred for 15 minutes. Then, 201 parts of deionized water were added dropwise while stirring for 1 hour to obtain an acrylic modified epoxy resin No. 2 aqueous dispersion having an acid value of 44 mgKOH / g and a solid content of 30%.

[0129] Production of phenolic resin (D)

[0130] Preparation Example 6 Preparation of Phenolic Resin No. 1 Solution

[0131] In a glass four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet, 188 parts of phenol and 324 parts of a 37% formaldehyde aqueous solution were added and heated to 50°C to uniformly dissolve the contents. Next, zinc acetate was added, mixed and the pH value in the system was adjusted to 5.0, and then heated to 90°C for reaction for 5 hours. Then, the mixture was cooled to 50°C, 32% calcium hydroxide aqueous dispersion was slowly added, the pH value was adjusted to 8.5, and the mixture was reacted at 50°C for 4 hours.

[0132] After the reaction, the pH value was adjusted to 4.5 with 20% hydrochloric acid, and the resin component was extracted with a mixed solvent of xylene / n-butanol / cyclohexane = 1 / 2 / 1 (mass ratio), the catalyst was removed, and the salt was neutralized, and then azeotropic dehydration was performed under reduced pressure to obtain a phenolic resin No. 1 solution with a solid content of 50%. The number average molecular weight of the resin solid content of the phenolic resin No. 1 solution was 350, and the average number of hydroxymethyl groups per benzene nucleus was 1.3.

[0133] Preparation Example 7 Preparation of Phenolic Resin No. 2 Solution

[0134] 108 parts of m-cresol, 216 parts of 37% formaldehyde aqueous solution and 160 parts of 25% sodium hydroxide aqueous solution were placed in a glass four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet, and reacted at 50°C under a nitrogen flow, then heated to 100°C and reacted for another hour; after neutralization with hydrochloric acid, the resin component was extracted with a mixed solvent of xylene / n-butanol = 1 / 1 (mass ratio), the catalyst and neutralization salt were removed, and then azeotropic dehydration was performed under reduced pressure to obtain a phenolic resin No. 2 solution with a solid content of 50%. The number average molecular weight of the resin solid content of the phenolic resin No. 2 solution is 350, and the average number of hydroxymethyl groups in each benzene nucleus is 0.7.

[0135] Production of waterborne coating compositions for cans

[0136] Example 1

[0137] In a container, 100 parts (solid content) of the acrylic modified epoxy resin No. 1 aqueous dispersion obtained in Preparation Example 4, 0.3 parts of refined palm oil (Note 2), 1 part of AB-50 (Note 9), and 3 parts (solid content) of the phenolic resin No. 1 solution obtained in Preparation Example 6 were uniformly mixed and adjusted with deionized water to obtain a can water-based coating composition No. 1 having a solid content of 30% by mass.

[0138] Examples 2 to 84 and Comparative Examples 1 to 65

[0139] Aqueous can coating compositions No. 2 to No. 149 were obtained in the same manner as in Example 1 except that the formulations were set as shown in Table 1. The results of tests conducted according to the following test methods are shown. The composition ratios in Table 1 are solid content mass ratios.

[0140] In addition, can water-based coating compositions Nos. 85 to 149 were used as comparative examples.

[0141] In addition, each notation in the table is as follows.

[0142] (Note 2) Refined palm oil: manufactured by Nissin Oil Refining Co., Ltd., palm oil, melting point 39°C;

[0143] (Note 3) Refined lanolin: manufactured by CRODA, lanolin wax, melting point 39°C;

[0144] (Note 4) HD-3028: Made by Gifu Shellac Manufacturing Co., Ltd., carnauba wax, melting point 82°C;

[0145] (Note 5) Hi-Mic-1070: manufactured by Nippon Seijo Co., Ltd., microcrystalline wax, melting point 80°C;

[0146] (Note 6) Lanco1370LF: manufactured by Lubrizol Corporation of Japan, polypropylene wax, melting point 150, average particle size 9 μm;

[0147] (Note 7) CERAFLOUR 991: manufactured by BYK, polyethylene wax, melting point 115, average particle size 5 μm;

[0148] (Note 8) CERAFLOUR 913: manufactured by BYK, trade name, polypropylene wax, melting point 160, average particle size 18 μm;

[0149] (Note 9) AB-50: manufactured by Gifu Shellac Manufacturing Co., Ltd., with an average particle size of 1 μm and a needle penetration of 1 to 2.

[0150] (Note 10) A-375: manufactured by Gifu Shellac Manufacturing Co., Ltd., with an average particle size of 2 μm and a needle penetration of 1 to 2.

[0151] (Note 11) A-110: manufactured by Gifu Shellac Manufacturing Co., Ltd., with an average particle size of 5 μm and a needle penetration of less than 1.

[0152] (Note 12) CHEMIPEARL W300: manufactured by Mitsui Chemicals, Inc., average particle size 3 μm, needle penetration less than 1;

[0153] (Note 13) CHEMIPEARL W500: manufactured by Mitsui Chemicals, Inc., average particle size: 2.5 μm, needle penetration: 10;

[0154] (Note 14) CHEMIPEARL F640: manufactured by Mitsui Chemicals, Inc., average particle size: 1 μm, needle penetration: 10;

[0155] [In addition, (Note 9) to (Note 14) are polyolefin dispersions]

[0156] (Note 15) NACURE 5225: manufactured by King Industries, USA. Trade name for an amine-neutralized solution of dodecylbenzenesulfonic acid.

[0157] (Note 16) NACURE 2500: a product of King Industries, Inc., USA. It is a product of an amine-neutralized solution of p-toluenesulfonic acid.

[0158]

[0159]

[0160]

[0161]

[0162]

[0163]

[0164]

[0165]

[0166]

[0167] Preparation of test board

[0168] The water-based coating compositions No. 1 to 149 obtained in the above examples and comparative examples were coated with a bar coater so that the dry coating weight reached 40 mg / 100 cm 2 The raw material was coated on an aluminum plate having a thickness of 0.26 mm in the form of a coating, and baked for 17 seconds using a dryer at an ambient temperature of 315° C. and a wind speed of 30 m / min in the form of a maximum temperature of 270° C. to obtain corresponding test plates.

[0169] The following evaluation items were tested and evaluated for each of the obtained test plates. The evaluation results are collectively shown in Table 1.

[0170] Coating appearance: The appearance of each test plate was evaluated visually. The smoothness, pitting and wrinkling of the coating surface were evaluated according to the following criteria:

[0171] ◎: The coating surface is smooth and has no pitting or wrinkles with a diameter of more than 1 mm;

[0172] ○: Tiny pitting and / or wrinkles with a diameter of more than 1 mm, and tiny orange peel wrinkles are visible;

[0173] △: Pits and / or wrinkles with a diameter of 1 mm or more are visible.

[0174] ×: Pockmarks and / or wrinkles with a diameter of 1 mm or more are clearly seen.

[0175] Processability: Cut the test plate 5cm in the rolling direction and 4cm in the vertical direction, and then fold the lower part in parallel with the short side. In a room at 20°C, clamp two aluminum plates with a thickness of 0.26mm between the bent parts of the test piece and place them on a special hemmed DuPont impact tester. Drop a 1kg iron weight with a flat contact surface from a height of 50cm, apply an impact to the bent part, and then apply a voltage of 6.5V to the front end of the bend for 6 seconds. Measure the current value (mA) of the 20mm width of the front end of the bend and evaluate according to the following criteria:

[0176] ◎: less than 10mA;

[0177] ○: greater than or equal to 10mA and less than 20mA;

[0178] △: 20mA or more and less than 40mA;

[0179] ×: 40mA or more.

[0180] Dynamic friction coefficient: On a test plate adjusted to 15 cm x 30 cm in size, a mass of 1 kg supported by three steel balls is placed and stretched at a speed of 150 cm / min to determine the dynamic friction coefficient (μ value). The smaller the dynamic friction coefficient (μ value), the better the sliding property.

[0181] ◎: μ value is less than 0.06;

[0182] ○: μ value is 0.06 or more and less than 0.1;

[0183] Δ: μ value is greater than 0.1 and less than 0.15;

[0184] ×: μ value is greater than or equal to 0.15.

[0185] Scratch resistance: The scratch resistance was evaluated by the load at which the test needle reaches the aluminum plate using a friction and wear tester TRIBOGEAR (manufactured by Shinto Scientific Co., Ltd., trade name, HEIDON-22H, test needle 150 μm, scratching speed 60 mm / min) for a test plate adjusted to a size of 10 cm × 20 cm:

[0186] ◎: The load of the test needle reaching the aluminum plate is above 300g;

[0187] ○: The load when the test needle reaches the aluminum plate is 200 g or more and less than 300 g;

[0188] △: The load when the test needle reaches the aluminum plate is greater than 150g and less than 200g;

[0189] ×: The load at which the test needle reaches the aluminum plate is less than 150 g.

[0190] Wear resistance: A friction test was conducted on a test plate adjusted to a size of 1.5 cm × 16 cm using a Bowden wear tester (manufactured by Kobelco, Ltd., Soda-type adhesion and sliding tester, friction part ball indenter 3 / 16 inch steel ball, load 4 kgf, friction speed 7 reciprocating / minute), and the number of frictions until the coating film was damaged was measured, and the evaluation was performed according to the following criteria:

[0191] ◎: No scratches were observed on the coating film after 50 rubbing times;

[0192] ○: The coating film is damaged when the number of frictions is 30 or more and 49 or less;

[0193] △: Scratches occur on the coating film when the number of frictions is 10 or more and 29 or less;

[0194] ×: When the number of rubbing is 9 times or less, scratches are generated on the coating film.

[0195] Industrial Applicability

[0196] According to the present invention, it is possible to provide a can body having a coating film excellent in sliding property, wear resistance and processability.

Claims

1. A water-based coating composition for cans, comprising an acrylic modified epoxy resin (A), a wax (B), a polyolefin aqueous dispersion (C) and a phenolic resin (D), characterized in that: The acrylic modified epoxy resin (A) is A resin (1) obtained by subjecting a bisphenol epoxy resin (a1) to an ester addition reaction with a carboxyl group-containing acrylic resin (a2), or A resin (2) obtained by graft-polymerizing a polymerizable unsaturated monomer component containing a carboxyl group-containing polymerizable unsaturated monomer with a bisphenol-type epoxy resin (a1); The wax (B) comprises at least one wax selected from the group consisting of a wax (b1) having a melting point lower than 50°C, a wax (b2) having a melting point of 50°C or higher and lower than 100°C, and a wax (b3) having a melting point of 100°C to 160°C and an average particle size of 1 μm to 15 μm, The average particle size of the polyolefin aqueous dispersion (C) is 0.1 μm to 5 μm, and the needle penetration of the polyolefin is 8 or less. Based on the total solid content of the acrylic modified epoxy resin (A), the total solid content of the wax (B) is 0.3% to 10% by mass, the total solid content of the polyolefin aqueous dispersion (C) is 1% to 10% by mass, and the total solid content of the phenolic resin (D) is 0.5% to 20% by mass.

2. The aqueous can coating composition according to claim 1, wherein the wax (b1) is at least one selected from the group consisting of lanolin wax, palm oil and triglyceride.

3. The aqueous can coating composition according to claim 1 or 2, wherein the wax (b2) is at least one selected from the group consisting of microcrystalline wax and carnauba wax.

4. The aqueous coating composition for cans according to claim 1 or 2, wherein the wax (b3) is at least one selected from the group consisting of polyethylene wax and polypropylene wax.

5. The aqueous coating composition for cans according to claim 1 or 2, wherein The solid content of the wax (b1), the wax (b2) and the wax (b3) is, based on the total solid content of the acrylic modified epoxy resin (A), 0.1% to 5% by mass of the wax (b1), 0.1% to 5% by mass of the wax (b2), and 0.1% to 5% by mass of the wax (b3).

6. The aqueous coating composition for cans according to claim 1 or 2, which is used for can covers. 7 . A can cap having a coating film of the aqueous coating composition for cans according to claim 1 .