Lead-free solder alloy and soldering method thereof

By adding S and Bi to the Sn-Zn lead-free solder alloy, its oxidation resistance and wettability are improved, and a simplified brazing process is used to solve the problem of poor corrosion resistance and poor corrosion resistance of Sn-Zn alloys in corrosive environments. Solve the problem of complex process and achieve efficient and low-cost brazing effect.

CN116140861BActive Publication Date: 2024-10-29NANCHANG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211622765.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-10-29
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

Existing lead-free solder alloys have poor corrosion resistance in corrosive environments, complex processes and high costs. In particular, Sn-Zn alloys have limited applications due to the easy oxidation of Zn and low corrosion potential.

Method used

Sn-Zn-S-Bi lead-free solder alloy is used. By adding S and Bi, the oxidation resistance and wettability of the alloy are improved, and powder and flux with a particle size of 20-50 μm are used during the soldering process to combine Brazing with heat and pressure simplifies the process and reduces porosity.

Benefits of technology

It improves the corrosion resistance and mechanical properties of solder alloys in different corrosive environments, reduces the melting point and cost of the alloy, simplifies the brazing process, and obtains dense and reliable joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004002734070000011
    Figure HDA0004002734070000011
  • Figure HDA0004002734070000012
    Figure HDA0004002734070000012
  • Figure HDA0004002734070000021
    Figure HDA0004002734070000021
Patent Text Reader

Abstract

The present invention discloses a lead-free solder alloy and a soldering method thereof, and relates to the technical field of metal materials. The components of the lead-free solder are: Zn 3‑15wt.%, Bi 0.5‑6wt.%, S 0.005‑0.8wt.%, Sr 0.001‑2wt.%, and the remainder is Sn. The soldering method of the present invention is: after ball-milling and mixing each raw material powder with a particle size of 20‑50μm, a small amount of flux is added, and after stirring, it is pre-pressed into thin blocks, placed between clean Cu or Ag substrates to be welded, and then a pressure of 5‑15MPa is vertically applied to the surface of the substrate while heating, and the mixture is cooled and solidified after being kept warm for 1‑10min. The S in the present invention can improve the oxidation resistance and corrosion resistance of the alloy; adding an appropriate amount of Bi may interact with S to form Bi 2 S 3 , improving its corrosion resistance and mechanical properties; Sr has a strong affinity with oxygen, which can reduce the oxygen content in the solder alloy and refine the microstructure of the Sn-Zn matrix. The brazing process has low temperature, simple process, low cost of solder alloy, and is suitable for soft soldering of metal materials such as Cu and Ag in electronic packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal materials, in particular to a lead-free solder alloy and a soldering method thereof. Background Art

[0002] With the vigorous development of the electronics industry and the increasing concern of human beings for health and environmental awareness, electronic products are becoming increasingly miniaturized and lightweight, and the three-dimensional and high-density electronic packaging has led to increasing requirements for the reliability of lead-free solder joints. It is urgent to develop new lead-free solders with excellent comprehensive performance and simple and reliable welding process.

[0003] In this context, binary and ternary lead-free solder alloys such as Sn-Zn, Sn-Cu, Sn-Ag, Sn-Ag-Cu have been studied and developed, and later quaternary alloys were developed on their respective bases. The Sn-Ag-Cu alloys in the Sn-Ag alloy series have been studied quite maturely in Europe, the United States, Japan and other places, and are expected to become one of the development directions of lead-free solders, but their disadvantages are high cost and melting point as high as 217℃, far exceeding the 183℃ of Sn-Pb; Sn-Cu alloys are low in cost and widely used in wave soldering, but the problems are high melting point and poor mechanical properties. The more effective solution is to add alloy elements such as Ni, Al and Ag. The eutectic melting point of Sn-Zn alloy is 198.5℃, which is close to the melting point of eutectic Sn-Pb, and it is compatible with existing process equipment, has excellent mechanical properties, low cost, and has good application prospects. However, Zn is more active and easily oxidized, and is easily corroded due to its low corrosion potential, which greatly hinders the spreading of the alloy on the substrate to be soldered and causes the joint to fail due to poor corrosion resistance in corrosive media environments. At present, the performance of Sn-based lead-free solder alloys is mainly improved by adding alloying elements such as RE, In, Bi, Al, P, Ag, Cu, Ga, and Cr. Although the development of Sn-Zn lead-free solder has achieved certain results, as the service conditions of connectors become increasingly harsh, its wettability and oxidation resistance are still difficult to match those of Sn-Pb solder, and its corrosion resistance in corrosive environments is not enough, and its application and development have encountered great obstacles.

[0004] The preparation method of solder alloy is basically to prepare by smelting method, and then to process into powder, wire, rod, strip of required shape through multiple processes, and finally to braze by various brazing processes, which is complicated, has long production cycle and high cost. When preparing Sn-based lead-free solder alloy by smelting method, especially when containing alloy components that are easy to oxidize and burn, more complex and effective anti-oxidation and burning means are required, which increases the process steps and difficulty. At the same time, high melting point intermetallic compounds are easily formed during smelting, and there are many oxidation inclusions. At present, it is reported that lead-free solder alloy is prepared by powder metallurgy method, which can avoid the formation of high melting point intermetallic compounds during smelting to a certain extent, but it needs to be pressed and sintered to obtain the required alloy, and then brazed by various brazing methods, which is relatively complicated. Summary of the invention

[0005] The object of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a Sn-Zn-S-Bi lead-free solder alloy and a soldering method thereof.

[0006] The technical solution of the present invention is as follows:

[0007] A lead-free solder alloy, the components and their mass percentages of which are: 3-15wt.%, 0.5-6wt.%, 0.005-0.8wt.%, and the balance is Sn.

[0008] As a preferred embodiment of the present invention, 0.001-2 wt. % of Sr is also included.

[0009] The present invention also discloses a method for soldering a Sn-Zn-S-Bi lead-free solder alloy, comprising the following steps: uniformly mixing raw materials Sn, Zn, Bi powder, S powder or Sn-S master alloy powder, adding flux, fully stirring and pre-pressing into thin blocks, placing the blocks between substrates to be soldered, applying vertical pressure on the surfaces of the substrates while heating, keeping the heat for 1-10 minutes and then cooling and solidifying to complete the soldering.

[0010] As a preferred embodiment of the present invention, the particle size of the Sn, Zn and Bi powders is 20-50 μm.

[0011] As a preferred embodiment of the present invention, at least one of Sr powder, Sn—Sr master alloy powder, and Zn—Sr master alloy powder is further added to the raw material.

[0012] As a preferred embodiment of the present invention, the pressure is 5-15 MPa.

[0013] As a preferred embodiment of the present invention, the heating is performed to a temperature in the range of 220-280°C.

[0014] As a preferred embodiment of the present invention, the substrate is Cu and / or Ag.

[0015] As a preferred embodiment of the present invention, the soldering flux is a mixture of rosin, ethanol, DMA and ethylene glycol.

[0016] As a preferred embodiment of the present invention, the amount of the soldering flux added is 1-20wt.% of the powder raw material.

[0017] The beneficial effects of the present invention are:

[0018] (1) The solder alloy of the present invention can improve the oxidation resistance and wettability of the Sn-Zn solder alloy by adding an appropriate amount of S, and at the same time can improve the corrosion resistance of the solder alloy in different corrosive environments; S may exist in two states in the Sn-Zn solder alloy, one part of which is the solid solution state S that easily combines with O to form SO2 or SO3 and escapes from the system; the other part of S is easily adsorbed and migrated to the more active Zn phase, interacts with Zn, and refines the Zn-rich phase. In addition, when corrosion occurs, it has a certain "pinning" effect on the Zn phase, thereby making it more difficult for selective corrosion of Zn to occur, thereby improving the corrosion resistance of the lead-free solder alloy; in addition, Bi can effectively reduce the melting point of the alloy and improve the wettability of the alloy on the one hand, and can be dissolved in the Sn-Zn solder matrix on the other hand, and may interact with S to form Bi2S3, thereby improving its corrosion resistance and mechanical properties.

[0019] (2) The Sr in the lead-free solder alloy of the present invention is an active metal with a strong affinity for oxygen, which can reduce the oxygen content in the solder alloy and further refine the microstructure of the Sn-Zn matrix. The alloy elements Bi, Sr and S used in the present invention are not rare elements and are low in cost.

[0020] (3) The brazing method of the present invention comprises the following steps: using Sn, Zn, Bi, Sr powder or Sn-Sr master alloy powder or Zn-Sr master alloy powder, S powder or Sn-S master alloy powder with a particle size of 20-50 μm, mixing the mixture evenly, adding 1-20 wt.% of flux, stirring the mixture thoroughly and pre-pressing the mixture into thin blocks, placing the blocks between clean Cu or Ag substrates to be welded, and then applying a pressure of 5-15 MPa vertically on the surfaces of the substrates while heating the blocks, keeping the heat for 1-10 minutes, and then cooling and solidifying the blocks to complete the brazing. The process of the present invention is simple and easy to operate. Pressurizing the blocks while heating the blocks can reduce the porosity of the brazed joints and welding defects, thereby obtaining dense and reliable brazed joints, thereby solving the problem of high-temperature steps of sintering or melting the brazing alloys used in the conventional brazing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a cross-section grinding metallographic image of the sample of Example 1;

[0022] Figure 2 The bar graph shows the relationship between the addition of S, Bi and Sr elements and the shear strength of the brazing specimens.

[0023] Figure 3 It is the relationship curve of different Bi contents on the wettability of samples;

[0024] Figure 4 It is a curve chart showing the relationship between weight loss of different samples and different immersion time;

[0025] Figure 5 Polarization curves of different samples. DETAILED DESCRIPTION

[0026] In order to solve the problems of poor wettability, oxidation resistance and corrosion resistance in Sn-Zn alloy, the wettability, mechanical properties and corrosion resistance of Sn-Zn alloy are improved by adding appropriate amounts of S, Bi and Sr, and soft soldering of Cu or Ag is achieved through a simple and convenient brazing process to reduce costs.

[0027] The present invention is achieved by the following technical solution. The lead-free solder alloy components and their mass percentages of the present invention are:

[0028] The Zn content is 3-15wt.%, the Bi content is 0.5-6wt.%, the S content is 0.005-0.8wt.%, and the balance is Sn.

[0029] In some applications, Sr content of 0.001-2 wt.% may be included.

[0030] The brazing method of the brazing alloy of the present invention is as follows: after uniformly mixing Sn, Zn, Bi powder, S powder or Sn-S master alloy powder with a raw material particle size of 20-50 μm, adding 1-20 wt.% of flux, fully stirring and pre-pressing into thin blocks, placing between clean Cu or Ag substrates to be welded, and then heating to a temperature range of 220-280° C., while vertically applying a pressure of 5-15 MPa on the surface of the substrate, keeping the temperature for 1-10 minutes, and then cooling and solidifying to complete the brazing.

[0031] At least one of Sr powder, Sn—Sr master alloy powder, and Zn—Sr master alloy powder may be added to the raw material.

[0032] The proper addition of S can improve the oxidation resistance and wettability of Sn-Zn solder alloy, and at the same time improve the corrosion resistance of solder alloy in different corrosive environments; S exists in two states in the Sn-Zn solder alloy. One part is the solid solution state S which is easy to combine with O to form SO2 or SO3 and escape from the system; the other part of S is easy to be adsorbed and migrated to the more active Zn phase, interact with the Zn phase, and refine the Zn-rich phase. In addition, when corrosion occurs, it has a certain pinning effect on the Zn phase, thereby making it more difficult for Zn to selectively corrode, thereby improving the corrosion resistance of lead-free solder alloy; Bi can effectively reduce the melting point of the alloy and improve the wettability of the alloy on the one hand, and on the other hand, it can be dissolved in the Sn-Zn solder matrix and may interact with S to form Bi2S3, thereby improving its corrosion resistance and mechanical properties; Sr is an active metal with a strong affinity for oxygen, which can reduce the oxygen content in the solder alloy. In addition, Sr can also refine the microstructure of the Sn-Zn matrix. The alloy elements Bi, Sr and S used in the present invention are not rare elements and have low cost.

[0033] After mixing evenly with Sn, Zn, Bi powder, Sr powder or Sn-Sr master alloy powder or Zn-Sr master alloy powder, S powder or Sn-S master alloy powder with a particle size of 20-50 μm, 1-20 wt.% flux is added, fully stirred and pre-pressed into thin blocks, placed between Cu or Ag substrates to be welded, and then heated while applying a pressure of 5-15 MPa vertically on the surface of the substrate, and then cooled and solidified after keeping warm for 1-10 minutes to complete brazing. The process is simple, the operation is easy, and a reliable brazing joint can be obtained.

[0034] The present invention will be further illustrated by the following examples.

[0035] Example 1

[0036] Sn, Zn, Bi powders with a particle size of 30 μm, Sn-S and Sn-Sr master alloy powders with a particle size of 25 μm, the mass percentage of Zn is 8%, the mass percentage of Bi is 2%, the mass percentage of Sn-S master alloy is based on the S content of 0.06%, the mass percentage of Sn-Sr master alloy is based on the Sr content of 0.2%, and the rest is Sn. After mixing evenly in a ball mill, add 8% (70wt.% rosin + 25wt.% ethanol + 2wt.% DMA + 3wt.% ethylene glycol) of flux, stir thoroughly, pre-press it into thin blocks, place it between the Cu substrates to be welded, and then heat it from room temperature to 250°C. While heating, apply a pressure of 10MPa vertically on the surface of the substrate. After keeping warm for 5 minutes, cool and solidify, complete brazing, and obtain a brazed connection. Take a cross-section of this sample and grind the metallographic structure ( Figure 1As shown in the figure, it can be seen that a continuous layer of intermetallic compound layer with a thickness of about 1-2 μm is formed at the interface of the solder joint after brazing, and the solder joint is dense, indicating that this process can achieve good welding between Cu substrates.

[0037] Example 2

[0038] Sn and Zn powders with a particle size of 25 μm, with the mass percentage of Zn being 6% and the balance being Sn, are used. After the alloy powders are mixed evenly in a ball mill, 10 wt.% (70 wt.% rosin + 25 wt.% ethanol + 2 wt.% DMA + 3 wt.% ethylene glycol) of flux is added, stirred thoroughly, pre-pressed into thin blocks, placed between Cu substrates to be welded, and then heated from room temperature to 255°C. While heating, a pressure of 8 MPa is applied vertically to the surface of the substrates. After keeping warm for 6 minutes, the blocks are cooled and solidified to obtain brazing parts of solder Sn-6Zn.

[0039] Example 3

[0040] Sn and Zn powders with a particle size of 25 μm were used, the mass percentage of Zn was 6%, the mass percentage of Sn-S master alloy was 0.06% S content, and the balance was Sn. The rest was the same as in Example 2, and a Sn-6Zn-0.06S brazing part was obtained.

[0041] Example 4

[0042] Sn and Zn powders with a particle size of 25 μm were used, with the mass percentage of Zn being 6%, the mass percentage of Bi being 1%, the mass percentage of the Sn-S master alloy being 0.06% S and the remainder being Sn, and the rest being the same as in Example 2, to obtain a Sn-6Zn-0.06S-1Bi brazing part.

[0043] Example 5

[0044] Sn and Zn powders with a particle size of 25 μm were used, with the mass percentage of Zn being 6%, the mass percentage of Bi being 1%, the mass percentage of the Sn-S master alloy being based on an S content of 0.06%, the mass percentage of the Sn-Sr master alloy being based on an S content of 0.5%, and the remainder being Sn. The rest was the same as in Example 2, to obtain a Sn-6Zn-0.06S-1Bi-0.5Sr brazing part.

[0045] Shear tensile tests were carried out on the brazed parts of Examples 2-5, and the results showed that the shear strengths of the four welded joints of Cu / Sn-6Zn / Cu, Cu / Sn-6Zn-0.06S / Cu, Cu / Sn-6Zn-0.06S-1Bi / Cu, and Cu / Sn-6Zn-0.06S-1Bi-0.5Sr / Cu were 35.3 MPa, 37.6 MPa, 40.5 MPa, and 44.2 MPa, respectively, indicating that with the addition of appropriate amounts of S, Bi, and Sr, the strength of the joint increases, as shown in FIG. Figure 2 shown.

[0046] Example 6

[0047] Sn, Zn, Bi alloy and Sn-S master alloy with a purity of 99.5% were used as raw materials, the mass percentage of Zn was 6.5%, the mass percentage of Sn-S master alloy was based on S content of 0.08%, the mass percentages of Bi were 0, 1%, 2%, 3%, 4%, and the rest was Sn. Five solder alloys with different Bi contents, Sn-6.5Zn-0.08S, Sn-6.5Zn-0.08S-1Bi, Sn-6.5Zn-0.08S-2Bi, Sn-6.5Zn-0.08S-3Bi, and Sn-6.5Zn-0.08S-4Bi, were prepared by smelting in a pit furnace, and wetting experiments were carried out to test their wetting spreading areas on a Cu substrate. The results are as follows: Figure 3 As shown, it can be seen that with the increase of Bi content, the wetting area of ​​the solder increases.

[0048] Example 7

[0049] Sn, Zn, Bi alloys with a purity of 99.5% and Sn-S and Sn-Sr master alloys were used as raw materials, with the mass percentage of Zn being 8% and the mass percentage of Bi being 3%. The mass percentages of the Sn-S master alloy were calculated based on S contents of 0.02% and 0.2%, respectively, and the mass percentage of the Sn-Sr master alloy was calculated based on Sr content of 0.3%, with the remainder being Sn. Sn-8Zn-3Bi, Sn-8Zn-3Bi-0.02S, Sn-8Zn-3Bi-0.2S, and Sn-8Zn-3Bi-0.02S-0.3Sr were respectively smelted in a pit furnace and cast into solder alloys. An immersion corrosion experiment was carried out to test the corrosion weight loss of the solder alloy under alkaline conditions with a pH value of about 10. The results are as follows: Figure 4 As shown, it can be seen that the weight loss of Sn-8Zn-3Bi solder alloy decreases with the addition of S and Sr content, indicating that its corrosion resistance in this environment is significantly improved.

[0050] Example 8

[0051] Using Sn, Zn, Bi alloys with a purity of 99.5% and Sn-S, Sn-Sr master alloys as raw materials, the mass percentage of Zn is 7%, the mass percentage of Bi is 1%, the mass percentage of Sn-S master alloy is based on S content of 0.05%, the mass percentage of Sn-Sr master alloy is based on S content of 0.2%, and the balance is Sn. Sn-7Zn-0.05S, Sn-7Zn-0.05S-1Bi, and Sn-7Zn-0.05S-1Bi-0.2Sr are smelted in a pit furnace respectively, cast into solder alloys, and electrochemical corrosion experiments are carried out. The polarization curves of the solder alloys in 3.5wt.% NaCl solution are tested. The results are as follows Figure 5 As shown in Table 1, the corresponding self-corrosion potential and corrosion current of the solder alloy are listed. Figure 5 It can be clearly seen from Table 1 that the addition of Bi and Sr elements can respectively increase the self-corrosion potential of the Sn-7Zn-0.05S solder alloy and reduce the corrosion current of the solder alloy, indicating that the corrosion resistance of the Sn-7Zn-0.05S solder alloy in 3.5wt.% NaCl solution is significantly improved.

[0052] Table 1 is composed of Figure 5 Electrochemical parameters obtained from the polarization curves shown

[0053] Alloy composition <![CDATA[Self - corrosion potential (E corr , V)]]> <![CDATA[Corrosion current (I corr , μA·cm -2 )]]> Sn-7Zn-0.05S -1.09 5.17 Sn-7Zn-0.05S-1Bi -1.02 4.82 Sn-7Zn-0.05S-1Bi-0.2Sr -0.95 1.56

[0054] Under the premise that no conflict occurs, those skilled in the art may freely combine and superimpose the above-mentioned additional technical features.

[0055] The above description is only a preferred embodiment of the present invention. Any technical solution that achieves the purpose of the present invention by substantially the same means belongs to the protection scope of the present invention.

Claims

1. A lead-free solder alloy, characterized in that: Its components and their mass percentages are: Zn content 3-15wt.%, Bi content 0.5-6wt.%, S content 0.005-0.8wt.%, and the balance is Sn; and it also includes 0.2-0.5wt.% Sr.

2. A method for soldering a lead-free solder alloy as claimed in claim 1, characterized in that: The method comprises the following steps: uniformly mixing raw materials of Sn, Zn, Bi powder and S powder or Sn-S master alloy powder, adding flux, stirring and pre-pressing into thin blocks, placing between substrates to be welded, and then heating while applying vertical pressure on the substrate surface, keeping the temperature for 1-10 minutes and then cooling and solidifying to complete the brazing.

3. The method for soldering a lead-free solder alloy according to claim 2, characterized in that: The particle size of the Sn, Zn and Bi powders is 20-50 μm.

4. The method for soldering a lead-free solder alloy according to claim 2, characterized in that: At least one of Sr powder, Sn-Sr master alloy powder and Zn-Sr master alloy powder is also added to the raw material.

5. The method for soldering a lead-free solder alloy according to claim 2, characterized in that: The pressure is 5-15 MPa.

6. A method for soldering a lead-free solder alloy according to claim 2, characterized in that: The substrate is Cu and / or Ag.

7. A method for soldering a lead-free solder alloy according to claim 2, characterized in that: The heating is to a temperature range of 220-280°C.

8. The method for soldering a lead-free solder alloy according to claim 2, characterized in that: The soldering flux is a mixture of rosin, ethanol, DMA and ethylene glycol.

9. The method for soldering a lead-free solder alloy according to claim 2, characterized in that: The added amount of the soldering flux is 1-20wt.% of the powder raw material.

Citation Information

Patent Citations

  • High-strength tin cadmium lead-free solder alloy and preparation method thereof

    CN102500947A

  • Method for preparing copper-aluminum bimetallic material through low-temperature diffusion

    CN109226992A

  • Lead-Free Solder Alloys Containing Sulfur and Their Manufacturing Methods