A TPU composite decorative film

By using specific components and processes in the protective layer of the TPU composite decorative film, its weather resistance and wear resistance are improved, the problem of insufficient performance of the existing TPU decorative film is solved, and high-performance decorative film preparation is achieved.

CN116141799BActive Publication Date: 2024-10-01DONGGUAN XIONGLIN NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211652438.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-10-01
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

Existing TPU decorative films have poor weather resistance and wear resistance, making it difficult to meet the needs of high-performance decorative materials.

Method used

A TPU composite decorative film is designed, which improves the protective layer by using components such as polyester glycol, polyether glycol, silicone and fillers in the protective layer, combined with specific silicone materials and modified nanoparticles. Weather resistance and wear resistance, and a protective layer with excellent properties is prepared through polymerization and extrusion granulation processes.

Benefits of technology

It achieves better mechanical properties, weather resistance and wear resistance of TPU composite decorative film, with tensile strength of 59.1~60.5MPa, peel strength of 7.2~8.0N/cm, yellowing resistance up to level 8, and wear resistance It is 7.0~8.5mg.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004011137140000131
    Figure BDA0004011137140000131
  • Figure BDA0004011137140000141
    Figure BDA0004011137140000141
Patent Text Reader

Abstract

The present invention provides a TPU composite decorative film. The TPU composite decorative film comprises a protective layer, a pattern layer and a substrate layer which are sequentially stacked; the raw materials for preparing the protective layer comprise the following components in parts by weight: 20 to 40 parts of polyester diol, 10 to 30 parts of polyether diol, 25 to 40 parts of diisocyanate, 3 to 15 parts of chain extender, 3 to 10 parts of organosilicon and 1 to 5 parts of filler. The present invention prepares a TPU composite decorative film with good mechanical properties, good weather resistance and good wear resistance by designing the raw materials for preparing the protective layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of decorative materials, and in particular relates to a TPU decorative material. Background Art

[0002] With the advancement of science and technology and the improvement of living standards and aesthetic tastes, people's demand for improving the quality of life is becoming more and more urgent, the requirements for decorative materials are becoming higher and higher, and the pursuit of personalized quality of product appearance is becoming more and more diverse. Decorative film materials, as a widely used decorative material, came into being under such circumstances. This material mainly plays a decorative and protective role. In addition to its aesthetic effect, it also has some other properties, such as heat insulation, warmth retention, UV protection, safety, explosion-proof, anti-theft, bulletproof and privacy. Developing decorative film materials with excellent performance can effectively improve the appearance of products, give people a sense of beauty, improve people's aesthetic comfort, and meet people's personalized needs for decorative materials.

[0003] At present, the most common decorative film is PVC decorative film, which can make the surface of the decorated object have a higher hardness, prevent the surface from being artificially scratched, abraded or bumped, thereby better protecting the decorated object and increasing its service life.

[0004] CN109280289A discloses a zero shrinkage decorative film, and its raw material composition is as follows: 100 parts of PVC sizing material, 6-12 parts of zinc powder, 2-3 parts of epoxy soybean oil, 2-6 parts of nano calcium carbonate, 5-10 parts of titanium dioxide, 2-6 parts of colorant, 20-40 parts of plasticizer, 2-4 parts of cadmium barium zinc composite stabilizer and 20-40 parts of processing aids by weight ratio. Through the formula, especially the addition of processing aids, the decorative film is made to have zero shrinkage and the service life of the decorative film is extended, but the material composition is relatively complex and the amount of additives added is relatively large. In the long-term use process, these additives are easy to seep out from the base material, thereby affecting the service life of the material, and it does not have the function of absorbing ink, and does not improve the clarity and firmness of the printed layer image and text.

[0005] CN105482548A discloses an environmentally friendly PVC decorative film and a preparation method thereof. The environmentally friendly PVC decorative film comprises an environmentally friendly PVC substrate, a water-based ink printing layer printed on the environmentally friendly PVC substrate, and an environmentally friendly PVC mask pressed on the water-based ink printing layer; the water-based ink is an inorganic nano-modified acrylate composite coating, and the raw material components mainly include: 18-22 parts of nano-silicon dioxide acrylate composite emulsion, 42-55 parts of self-crosslinking styrene-acrylic emulsion, 20-32 parts of high solid content pigment filter cake, 0.3-0.8 parts of defoamer, 0.6-1.2 parts of wetting and leveling agent, 0.3-0.8 parts of thickener, 0.5-1.2 parts of transfer aid, 0.3-1 parts of anionic surfactant, 1-4 parts of industrial alcohol and 1-2 parts of water. The environmentally friendly PVC decorative film has the excellent properties of being non-toxic, tasteless and having good thermal stability.

[0006] In the prior art, although PVC decorative films with different excellent properties have been prepared, the weather resistance, high temperature resistance, wear resistance, etc. of the prepared PVC decorative films need to be further improved.

[0007] Thermoplastic polyurethane elastomer (TPU) is a linear polymer material generated by the reaction of diisocyanate, oligomer polyol and chain extender. It is characterized by repeated urethane groups in molecular composition, and contains other groups such as allophanate, biuret, ester bond, ether bond, etc.; from the perspective of molecular structure, it is composed of alternating rigid segments and flexible segments, in which the rigid segments are obtained by the reaction of diisocyanate and chain extender, and the flexible segments are obtained by the reaction of diisocyanate and macromolecular polyol. This special molecular structure makes TPU have excellent properties that are incomparable to other types of thermoplastic elastomers, but its weather resistance is poor.

[0008] Therefore, how to prepare a TPU composite decorative film with excellent properties such as wear resistance and weather resistance through TPU has become a technical problem that needs to be solved urgently. Summary of the invention

[0009] In view of the shortcomings of the prior art, the present invention aims to provide a TPU composite decorative film. In the present invention, by designing the structure of the TPU composite decorative film and further designing the raw materials for preparing the protective layer, a TPU composite decorative film with good mechanical properties, good weather resistance and good wear resistance is prepared.

[0010] To achieve this object, the present invention adopts the following technical solutions:

[0011] The present invention provides a TPU composite decorative film, which comprises a protective layer, a pattern layer and a substrate layer which are sequentially stacked;

[0012] The raw materials for preparing the protective layer include the following components in parts by weight: 20-40 parts of polyester diol, 10-30 parts of polyether diol, 25-40 parts of diisocyanate, 3-15 parts of chain extender, 3-10 parts of silicone, and 1-5 parts of filler.

[0013] In the present invention, by designing the structure of the TPU composite decorative film and further designing the raw materials for preparing the protective layer, and by using polyester diol and polyether diol, the TPU composite decorative film has both good mechanical properties and good softness; at the same time, by using silicone, the silicone modifies the polyurethane molecular chain to make it have good weather resistance, and by using fillers, the wear resistance of the TPU protective layer can be further improved.

[0014] In the present invention, the weight proportions of the polyether diol may be 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts or 40 parts, etc.

[0015] The weight proportions of the polyester diol may be 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts or 30 parts, etc.

[0016] The weight parts of the diisocyanate can be 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts or 40 parts, etc.

[0017] The weight proportions of the chain extender can be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts, etc.

[0018] The weight proportions of the silicone may be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts, etc.

[0019] The weight proportion of the filler can be 1 part, 2 parts, 3 parts, 4 parts or 5 parts.

[0020] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0021] As a preferred technical solution of the present invention, the organosilicon is selected from aminodimethylsiloxane and / or polytrifluoropropylmethylsiloxane, preferably a combination of aminodimethylsiloxane and polytrifluoropropylmethylsiloxane.

[0022] Preferably, the mass ratio of the terminal aminodimethylsiloxane to the polytrifluoropropylsiloxane is 1:(0.5-1), for example, it can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:1.

[0023] In the present invention, by selecting a specific organic silicon material, preferably a combination of amino-terminated dimethylsiloxane (PDMS) and polytrifluoropropylsiloxane (PMTFPS), the yellowing resistance of the prepared protective layer is good by using the two materials together and controlling the mass ratio of the two materials within a specific range. If the mass ratio of the two materials is too large or too small, the yellowing resistance of the prepared protective layer is poor.

[0024] In the present invention, by using terminal aminodimethylsiloxane and polytrifluoropropylsiloxane, silicon atoms and fluorine atoms can be introduced into the polyurethane molecular chain, thereby improving the yellowing resistance of the protective layer, and by reducing the polarity of the polyurethane molecular weight, the stain resistance of the protective layer can be improved.

[0025] As a preferred technical solution of the present invention, the filler is modified inorganic particles.

[0026] Preferably, the filler has a D 50 The particle size is 10 to 100 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.

[0027] Preferably, the inorganic particles are selected from nano zinc oxide and / or nano aluminum oxide, and more preferably are a combination of nano zinc oxide and nano aluminum oxide.

[0028] In the present invention, by using modified nanoparticles, the compatibility of the nanoparticles with polyurethane can be improved, so that the nanoparticles are evenly dispersed in the protective layer, and the wear resistance of the protective layer is further improved.

[0029] In the present invention, the wear resistance of the protective layer can be effectively improved by using specific modified nanoparticles and further using modified nano zinc oxide and nano aluminum oxide in combination.

[0030] Preferably, the modifier of the modified inorganic particles is a silane coupling agent.

[0031] Preferably, the silane coupling agent is selected from KH550 (γ-aminopropyltriethoxysilane) and / or KH560 (γ-(2,3-epoxypropyloxy)propyltrimethoxysilane).

[0032] In the present invention, the preparation method of the modified inorganic particles is as follows:

[0033] The silane coupling agent and the organic solvent are mixed, and inorganic particles are added thereto under ultrasonic conditions. After the modification reaction is carried out at 20-40° C. for 12 hours, the mixture is centrifuged, washed with ethanol for three times, and ground to obtain the modified inorganic particles.

[0034] It should be noted that there is no special limitation on the use of the above-mentioned organic solvent in the present invention, and any organic solvent commonly used in the art is applicable, including but not limited to toluene.

[0035] As a preferred technical solution of the present invention, the number average molecular weight of the polyester diol is 300-4000, for example, it can be 300, 500, 1000, 1500, 2000, 2500, 3000, 3500 or 4000.

[0036] Preferably, the polyester diol is selected from any one of polybutylene adipate diol, polyethylene adipate diol, polyhexane adipate diol or polycaprolactone diol, or a combination of at least two thereof.

[0037] Preferably, the number average molecular weight of the polyether diol is 400-4000, for example, 400, 500, 700, 1000, 1200, 1500, 1800, 2000, 2700, 3000, 3200, 3500, 3800 or 4000.

[0038] Preferably, the polyether diol is polytetramethylene ether diol and / or polytetramethylene ether diol.

[0039] As a preferred technical solution of the present invention, the diisocyanate is an aliphatic diisocyanate.

[0040] In the present invention, by using aliphatic diisocyanate, the introduction of benzene ring structure into the polyurethane molecule is avoided, and the yellowing resistance of the protective layer can be improved.

[0041] Preferably, the diisocyanate is selected from any one of hexamethylene diisocyanate, 4,4-dicyclohexylmethane diisocyanate or isophorone diisocyanate, or a combination of at least two thereof.

[0042] Preferably, the chain extender is selected from any one of 1,2-ethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol or trimethylolpropane, or a combination of at least two thereof.

[0043] As a preferred technical solution of the present invention, the raw materials for preparing the protective layer also include 0.05 to 0.2 parts of catalyst, for example, 0.05 parts, 0.07 parts, 0.1 parts, 0.12 parts, 0.14 parts, 0.16 parts, 0.18 parts or 0.2 parts.

[0044] Preferably, the catalyst is selected from dibutyltin dilaurate and / or stannous isooctanoate.

[0045] As a preferred technical solution of the present invention, the raw materials for preparing the protective layer also include 0.5 to 2 parts of lubricant, for example, it can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts or 2 parts, etc.

[0046] Preferably, the lubricant is selected from any one of ethylene bisstearamide, erucamide or oleamide, or a combination of at least two thereof.

[0047] In the present invention, the method for preparing the protective layer comprises the following steps:

[0048] (1) After the polyester diol, polyether diol, silicone and diisocyanate are subjected to vacuum drying and dehydration treatment, they are mixed evenly, and a portion of the catalyst is added thereto, and a polymerization reaction is carried out at 70 to 80° C. for 3 to 5 hours to obtain a polyurethane prepolymer;

[0049] (2) The polyurethane prepolymer, chain extender, filler, remaining catalyst and optional lubricant obtained in step (1) are mixed, extruded into granules, dried, and then the TPU particles are melt-plasticized by a single-screw extruder, extruded and cast, and calendered to obtain the protective layer.

[0050] As a preferred technical solution of the present invention, an adhesive layer is provided between the pattern layer and the protective layer.

[0051] Preferably, the adhesive layer is prepared from an adhesive.

[0052] Preferably, the adhesive is selected from any one of polyacrylic adhesive, polyurethane adhesive, epoxy resin adhesive, or a combination of at least two thereof.

[0053] Preferably, the thickness of the adhesive layer is 0.05-0.2 mm, for example, 0.05 mm, 0.07 mm, 0.1 mm, 0.12 mm, 0.14 mm, 0.16 mm, 0.18 mm or 0.2 mm.

[0054] As a preferred technical solution of the present invention, the thickness of the protective layer is 0.05-2 mm, for example, it can be 0.05 mm, 0.1 mm, 0.2 mm, 0.4 mm, 0.6 mm, 0.8 mm, 1 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm or 2 mm.

[0055] As a preferred technical solution of the present invention, the thickness of the substrate layer is 0.1 to 2 mm, for example, it can be 0.1 mm, 0.2 mm, 0.4 mm, 0.6 mm, 0.8 mm, 1 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm or 2 mm.

[0056] It should be noted that there is no special limitation on the material of the substrate layer in the present invention, and all commonly used materials in the art are applicable, including but not limited to TPU substrate.

[0057] In the present invention, the preparation method of the TPU composite decorative film comprises the following steps:

[0058] (A) printing a pattern on either side of the substrate layer to obtain a pattern layer;

[0059] (B) coating an adhesive on the side of the pattern layer away from the substrate layer, placing a protective layer on the side of the adhesive away from the substrate layer, and compounding to obtain the TPU composite decorative film.

[0060] Compared with the prior art, the present invention has the following beneficial effects:

[0061] In the present invention, by designing the structure of the TPU composite decorative film and further designing the raw materials for preparing the protective layer, and by using specific silicone materials and fillers, the weather resistance and wear resistance of the protective layer are further improved. At the same time, the prepared TPU composite decorative film has good mechanical properties, a tensile strength of 59.1 to 60.5 MPa, a peel strength of 7.2 to 8.0 N / cm, yellowing resistance of up to level 8, and a wear resistance of 7.0 to 8.5 mg. DETAILED DESCRIPTION

[0062] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0063] The sources of some components in the embodiments and comparative examples are as follows:

[0064] Polybutylene adipate diol: Jining Huakai Resin Co., Ltd.;

[0065] Polyethylene adipate glycol: Yantai Huada Chemical Industry Co., Ltd.;

[0066] Polycaprolactone diol: Japan Daicel Corporation, CAPA7201A;

[0067] Polytetramethylene glycol: BASF, PTMG1000;

[0068] Polytetramethylene ether glycol: DuPont, USA;

[0069] Aminopropyl-terminated polydimethoxysiloxane (PDMS): Chengdu Gracey Chemical Technology Co., Ltd.;

[0070] Polytrifluoropropylmethylsiloxane: CAS No.: 63148-56-1;

[0071] Nano zinc oxide: Nanophase Technologies, USA;

[0072] Nano-alumina: Guangzhou Yanrui Chemical Co., Ltd.;

[0073] Epoxy resin adhesive: Shenzhen Nanbao glue;

[0074] TPU substrate: Dongguan Xionglin New Materials Technology Co., Ltd., thickness is 2mm.

[0075] The preparation method of the nano zinc oxide used in the following examples and comparative examples is as follows:

[0076] KH550 (5 g) and toluene (200 mL) were mixed, and nano zinc oxide (20 g) was added thereto under ultrasonic conditions. After the modification reaction was carried out at 25° C. for 12 h, the mixture was centrifuged, washed with ethanol for 3 times, and ground to obtain the modified nano zinc oxide.

[0077] The preparation method of the nano-alumina used in the following examples and comparative examples is as follows:

[0078] KH560 (5 g) and toluene (200 mL) were mixed, and nano-alumina (20 g) was added thereto under ultrasonic conditions. After a modification reaction was carried out at 30° C. for 12 h, the mixture was centrifuged, washed with ethanol for 3 times, and ground to obtain the modified nano-alumina.

[0079] Example 1

[0080] This embodiment provides a TPU composite decorative film, wherein the TPU composite decorative film comprises a protective layer, a pattern layer and a TPU substrate layer which are stacked in sequence;

[0081] The raw materials for preparing the protective layer include the following components in parts by weight: 30 parts of polybutylene adipate diol, 30 parts of polytetramethylene ether diol, 25 parts of 1,6-hexamethylene diisocyanate, 10 parts of 1,2-ethylene glycol, 8 parts of organic silicon, 2 parts of modified nano zinc oxide and 2 parts of modified nano aluminum oxide, 0.1 parts of dibutyltin dilaurate and 2 parts of oleamide;

[0082] The organic silicon is composed of terminal amino dimethyl siloxane and polytrifluoropropyl siloxane in a mass ratio of 1:0.8.

[0083] The preparation method of the protective layer is as follows:

[0084] (1) After vacuum drying and dehydration treatment, polybutylene adipate diol, polytetramethylene glycol ether diol, silicone and 1,6-hexamethylene diisocyanate are uniformly mixed, and a portion of dibutyltin dilaurate (0.05 parts) is added thereto, and a polymerization reaction is carried out at 75° C. for 3 hours to obtain a polyurethane prepolymer;

[0085] (2) The polyurethane prepolymer obtained in step (1), 1,2-ethylene glycol, modified nano zinc oxide, modified nano aluminum oxide and the remaining dibutyl tin dilaurate and oleic acid amide are mixed, extruded into granules, dried, and then the TPU particles are melt-plasticized by a single-screw extruder, extruded and cast, and calendered to obtain a protective layer with a thickness of 1 mm.

[0086] The preparation method of the above TPU composite decorative film is as follows:

[0087] (A) printing a pattern on either side of the TPU substrate layer to obtain a pattern layer;

[0088] (B) coating an epoxy resin adhesive on the side of the pattern layer away from the substrate layer, placing a protective layer on the side of the adhesive away from the substrate layer, and compounding to obtain the TPU composite decorative film.

[0089] Example 2

[0090] This embodiment provides a TPU composite decorative film, wherein the TPU composite decorative film comprises a protective layer, a pattern layer and a TPU substrate layer which are stacked in sequence;

[0091] The raw materials for preparing the protective layer include the following components in parts by weight: 20 parts of polyethylene adipate glycol, 30 parts of polytetramethylene ether glycol, 30 parts of 4,4-dicyclohexylmethane diisocyanate, 5 parts of trimethylolpropane, 3 parts of organic silicon, 1 part of modified nano zinc oxide and 1 part of modified nano aluminum oxide, 0.05 parts of dibutyltin dilaurate and 1 part of erucamide;

[0092] The organic silicon is composed of terminal amino dimethyl siloxane and polytrifluoropropyl siloxane in a mass ratio of 1:0.7.

[0093] The preparation method of the protective layer is as follows:

[0094] (1) After vacuum drying and dehydration treatment, polyethylene adipate glycol, polytetramethylene ether glycol, silicone and 4,4-dicyclohexylmethane diisocyanate are uniformly mixed, and a portion of dibutyltin dilaurate (0.03 parts) is added thereto, and a polymerization reaction is carried out at 75° C. for 3 hours to obtain a polyurethane prepolymer;

[0095] (2) The polyurethane prepolymer obtained in step (1), trimethylolpropane, modified nano zinc oxide, modified nano aluminum oxide and the remaining dibutyl tin dilaurate and erucic acid amide are mixed, extruded into granules, dried, and then the TPU particles are melt-plasticized by a single-screw extruder, extruded and cast, and calendered to obtain a protective layer with a thickness of 0.05 mm.

[0096] The preparation method of the above TPU composite decorative film is as follows:

[0097] (A) printing a pattern on either side of the TPU substrate layer to obtain a pattern layer;

[0098] (B) coating an epoxy resin adhesive on the side of the pattern layer away from the substrate layer, placing a protective layer on the side of the adhesive away from the substrate layer, and compounding to obtain the TPU composite decorative film.

[0099] Example 3

[0100] This embodiment provides a TPU composite decorative film, wherein the TPU composite decorative film comprises a protective layer, a pattern layer and a TPU substrate layer which are stacked in sequence;

[0101] The raw materials for preparing the protective layer include the following components in parts by weight: 40 parts of polycaprolactone diol, 10 parts of polytetramethylene glycol, 40 parts of 1,6-hexamethylene diisocyanate, 15 parts of 1,4-butanediol, 10 parts of organic silicon, 2 parts of modified nano zinc oxide, 3 parts of modified nano aluminum oxide, 0.2 parts of dibutyltin dilaurate and 0.5 parts of ethylene bisstearamide;

[0102] The organic silicon is composed of terminal amino dimethyl siloxane and polytrifluoropropyl siloxane in a mass ratio of 1:0.7.

[0103] The preparation method of the protective layer is as follows:

[0104] (1) After vacuum drying and dehydration treatment, polycaprolactone diol, polytetramethylene glycol, silicone and 1,6-hexamethylene diisocyanate are uniformly mixed, and a portion of dibutyltin dilaurate (0.1 parts) is added thereto, and a polymerization reaction is carried out at 75° C. for 3 hours to obtain a polyurethane prepolymer;

[0105] (2) The polyurethane prepolymer obtained in step (1), 1,4-butanediol, modified nano zinc oxide, modified nano aluminum oxide and the remaining dibutyltin dilaurate and ethylene bisstearamide are mixed, extruded into granules, dried, and then the TPU particles are melt-plasticized by a single-screw extruder, extruded and cast, and calendered to obtain a protective layer with a thickness of 2 mm.

[0106] The preparation method of the above TPU composite decorative film is as follows:

[0107] (A) printing a pattern on either side of the TPU substrate layer to obtain a pattern layer;

[0108] (B) coating an epoxy resin adhesive on the side of the pattern layer away from the substrate layer, placing a protective layer on the side of the adhesive away from the substrate layer, and compounding to obtain the TPU composite decorative film.

[0109] Example 4

[0110] This embodiment provides a TPU composite decorative film, which is different from Embodiment 1 only in that the organic silicone is composed of terminal amino dimethyl siloxane and polytrifluoropropyl siloxane in a mass ratio of 1:0.5, and other conditions are the same as those in Embodiment 1.

[0111] Example 5

[0112] This embodiment provides a TPU composite decorative film, which is different from Embodiment 1 only in that the organic silicone is composed of terminal amino dimethyl siloxane and polytrifluoropropyl siloxane in a mass ratio of 1:1, and other conditions are the same as those in Embodiment 1.

[0113] Example 6

[0114] This embodiment provides a TPU composite decorative film, which is different from Embodiment 1 only in that the organic silicone is composed of terminal amino dimethyl siloxane and polytrifluoropropyl siloxane in a mass ratio of 1:0.3, and other conditions are the same as those in Embodiment 1.

[0115] Example 7

[0116] This embodiment provides a TPU composite decorative film, which is different from Embodiment 1 only in that the organic silicone is composed of terminal amino dimethyl siloxane and polytrifluoropropyl siloxane in a mass ratio of 1:1.2, and other conditions are the same as those in Embodiment 1.

[0117] Example 8

[0118] This embodiment provides a TPU composite decorative film, which is different from the embodiment 1 only in that the organic silicon is amino-terminated dimethylsiloxane, and other conditions are the same as those of the embodiment 1.

[0119] Example 9

[0120] This embodiment provides a TPU composite decorative film, which is different from the embodiment 1 only in that the organic silicon is polytrifluoropropylsiloxane, and other conditions are the same as those of the embodiment 1.

[0121] Example 10

[0122] This embodiment provides a TPU composite decorative film, which is different from Embodiment 1 only in that the raw materials for preparing the protective layer do not contain modified nano zinc oxide, the weight proportion of the modified nano aluminum oxide is 4 parts, and other conditions are the same as those in Embodiment 1.

[0123] Embodiment 11

[0124] This embodiment provides a TPU composite decorative film, which is different from Embodiment 1 only in that the raw materials for preparing the protective layer do not contain modified nano-aluminum oxide, the weight proportion of the modified nano-zinc oxide is 4 parts, and other conditions are the same as those in Embodiment 1.

[0125] Comparative Example 1

[0126] This comparative example provides a TPU composite decorative film, which is different from Example 1 only in that the raw materials for preparing the protective layer do not contain silicone, and other conditions are the same as those in Example 1.

[0127] Comparative Example 2

[0128] This comparative example provides a TPU composite decorative film, which is different from Example 1 only in that the raw materials for preparing the protective layer do not contain modified nano zinc oxide and modified nano aluminum oxide, and other conditions are the same as those in Example 1.

[0129] The performance of the TPU composite decorative films provided in the above embodiments and comparative examples was tested, and the testing method was as follows:

[0130] Tensile strength: GB / T 528-2009;

[0131] Peel strength: GB / T 2790;

[0132] Yellowing resistance: refer to standard HG1T3689-2001, place the sample strip in a 340nm UV light box at 60℃ for continuous irradiation for 16 to 8 hours, and measure the yellowing degree with ISO105 nine-level color change gray card according to standard GB250-2008.

[0133] Wear resistance: The leather was subjected to a wear resistance test in accordance with the standard GB / T 1768-2006 to test the quality of wear. The instrument used was TAKER wear resistance tester ((G`T 7012-T) High-speed Railway Testing Instrument Company, grinding wheel type CS-10 speed 60r / min, grinding wheel load 1000g) with 1000 friction turns, and the wear quality was measured with an analytical balance and the average of three sets of data was taken to obtain the result.

[0134] Table 1

[0135]

[0136]

[0137] It can be seen from the contents of Table 1 that the present invention further improves the weather resistance and wear resistance of the protective layer by designing the raw materials for preparing the protective layer and using specific silicone materials and fillers. At the same time, the prepared TPU composite decorative film has good mechanical properties, with a tensile strength of 59.1-60.5 MPa, a peel strength of 7.2-8.0 N / cm, a yellowing resistance of up to level 8, and a wear resistance of 7.0-8.5 mg.

[0138] Compared with Example 1, if the mass ratio of terminal amino dimethyl siloxane to polytrifluoropropyl siloxane is too large or too small (Examples 6-7), the weather resistance of the prepared TPU composite decorative film is poor.

[0139] Compared with Example 1, if only amino-terminated dimethylsiloxane or polytrifluoropropylsiloxane is selected as the organic silicon material (Examples 8-9), the yellowing resistance of the prepared TPU composite decorative film is poor.

[0140] Compared with Example 1, if only modified nano zinc oxide or modified nano aluminum oxide is used as the filler (Examples 10-11), the wear resistance of the prepared TPU composite decorative film is poor.

[0141] Compared with the embodiment period, if the raw materials for preparing the protective layer do not contain silicone (Comparative Example 1), the weather resistance of the prepared TPU composite decorative film is poor, and its yellowing resistance is only level 5; if the raw materials for preparing the protective layer do not contain filler (Comparative Example 2), the wear resistance of the prepared TPU composite decorative film is poor.

[0142] In summary, the present invention improves the weather resistance and wear resistance of the protective layer by designing the raw materials for preparing the protective layer and using specific organic silicon materials and fillers. At the same time, the prepared TPU composite decorative film has good mechanical properties.

[0143] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A TPU composite decorative film, characterized in that: The TPU composite decorative film comprises a protective layer, a pattern layer and a substrate layer which are stacked in sequence; The raw materials for preparing the protective layer include the following components in parts by weight: 20-40 parts of polyester diol, 10-30 parts of polyether diol, 25-40 parts of diisocyanate, 3-15 parts of chain extender, 3-10 parts of silicone and 1-5 parts of filler; The organosilicon is selected from a combination of aminodimethylsiloxane and polytrifluoropropylmethylsiloxane; The mass ratio of the amino-terminated dimethylsiloxane to the polytrifluoropropylmethylsiloxane is 1:(0.5-1); The filler is modified inorganic particles; The inorganic particles are selected from a combination of nano zinc oxide and nano aluminum oxide; The modifier of the modified inorganic particles is a silane coupling agent; The raw materials for preparing the protective layer also include 0.05-0.2 parts of catalyst; The catalyst is selected from dibutyltin dilaurate and / or stannous isooctanoate.

2. The TPU composite decorative film according to claim 1, characterized in that: The D of the filler 50 The particle size is 10~100nm.

3. The TPU composite decorative film according to claim 1, characterized in that: The number average molecular weight of the polyester diol is 300-4000.

4. The TPU composite decorative film according to claim 1, characterized in that: The polyester diol is selected from any one of polybutylene adipate diol, polyethylene adipate diol, polyhexane adipate diol or polycaprolactone diol, or a combination of at least two thereof.

5. The TPU composite decorative film according to claim 1, characterized in that: The number average molecular weight of the polyether diol is 400-4000.

6. The TPU composite decorative film according to claim 1, characterized in that: The polyether diol is polytetrahydrofuran ether diol and / or polytetramethylene ether diol.

7. The TPU composite decorative film according to claim 1, characterized in that: The diisocyanate is an aliphatic diisocyanate.

8. The TPU composite decorative film according to claim 1, characterized in that: The diisocyanate is selected from any one of 1,6-hexamethylene diisocyanate, 4,4-dicyclohexylmethane diisocyanate and isophorone diisocyanate, or a combination of at least two thereof.

9. The TPU composite decorative film according to claim 1, characterized in that: The chain extender is selected from any one of 1,2-ethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol or trimethylolpropane, or a combination of at least two thereof.

10. The TPU composite decorative film according to claim 1, characterized in that: The raw materials for preparing the protective layer also include 0.5 to 2 parts of lubricant.

11. The TPU composite decorative film according to claim 10, characterized in that: The lubricant is selected from any one of ethylene bisstearamide, erucamide or oleamide, or a combination of at least two thereof.

12. The TPU composite decorative film according to claim 1, characterized in that: An adhesive layer is arranged between the pattern layer and the protective layer.

13. The TPU composite decorative film according to claim 12, characterized in that: The adhesive layer is prepared from an adhesive.

14. The TPU composite decorative film according to claim 13, characterized in that: The adhesive is selected from any one of polyacrylic adhesive, polyurethane adhesive, epoxy resin adhesive, or a combination of at least two thereof.

15. The TPU composite decorative film according to claim 12, characterized in that: The thickness of the adhesive layer is 0.05-0.2 mm.

16. The TPU composite decorative film according to claim 1, characterized in that: The thickness of the protective layer is 0.05-2 mm.

17. The TPU composite decorative film according to claim 1, characterized in that: The thickness of the substrate layer is 0.1-2 mm.