A nitrogen-doped carbon nanotube and its preparation method and application
Through the combination of dielectric electrophoretic assembly and local Joule thermal doping, the problem of high contact resistance between carbon nanotubes and metal electrodes is solved, and efficient contact performance improvement and environmentally friendly doping effect is achieved. It is suitable for micro-nano devices and small-scale Manufacturing of chemical electronic devices.
Patent Information
- Application Number
- CN202310156895.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-21
AI Technical Summary
In the prior art, the contact resistance between carbon nanotubes and metal electrodes is high, resulting in high power consumption of nano devices that affect performance and service life. The existing doping methods have low effectiveness, poor controllability, high cost and pollution. Big problem.
The dielectric electrophoretic assembly method is used to assemble carbon nanotubes on metal electrodes, and nitrogen doping is introduced to reduce the contact resistance between the carbon nanotubes and the metal electrodes through a combination of local Joule thermal doping and vapor deposition.
It has achieved high-efficiency contact performance between carbon nanotubes and metal electrodes, reduced contact resistance, and is suitable for micro-nano devices manufacturing, and is simple, environmentally friendly and low-cost, which is suitable for the manufacturing and secondary processing of miniaturized electronic devices.
Smart Images

Figure CN116143107B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of manufacturing electronic components, and in particular to a nitrogen-doped carbon nanotube and a preparation method and application thereof. Background Art
[0002] Carbon nanotubes (CNTs) have become one of the hot research materials in small or portable electronic devices in recent years due to their advantages such as light weight, excellent electrical and thermal properties, and good chemical stability. Metals are commonly used electrodes or conductors in small or portable electronic devices. In order to reduce the weight of electronic devices and improve their electrical properties, carbon nanotubes are generally assembled or connected with metal electrodes in electronic devices. However, there is a problem of excessively high contact resistance between carbon nanotubes and metal electrodes, which not only causes high heat and power consumption in nanodevices, but also directly affects the performance and service life of carbon nanotube nanodevices.
[0003] At present, the methods for reducing the contact resistance of carbon nanotubes mainly include metal deposition, high-temperature annealing, ultrasonic nano-welding, heteroatom doping, etc. Among them, the metal deposition method is a method of using metal to surround the connection between the carbon nanotube and the metal electrode to increase the contact area between the metal electrode and the carbon nanotube, which is not conducive to reducing the weight and cost of small devices; the high-temperature annealing method is easy to damage the performance of the device and its controllability is poor; the ultrasonic nano-welding method is not mature enough in technology, and has the problems of low repeatability and high growth cost; the heteroatom doping method generally uses vapor deposition on the surface of the carbon nanotube to reduce the contact resistance of the carbon nanotube, and this method has the problem of low doping effectiveness.
[0004] In addition, the main structure of carbon nanotubes is a six-membered ring of carbon, and the carbon-carbon bond in the six-membered ring of carbon is highly stable. It is difficult for carbon nanotubes without defect sites to accommodate foreign doping atoms. It is usually necessary to introduce more defect sites and functional groups into carbon nanotubes with the help of acid and / or high temperature treatment to improve the effectiveness of carbon nanotube doping. However, these methods not only require a large amount of carbon nanotubes, but also have problems such as poor repeatability, large amount of waste liquid, and poor controllability. In the field of micro-nano devices, the amount of carbon nanotubes is usually very small; when the amount of carbon nanotubes is small, high temperature and acid treatment are easy to cause great damage to the structure of carbon nanotubes, greatly deteriorating the excellent performance of carbon nanotubes themselves, and also have an adverse effect on the performance of metal electrodes and device substrates (for example, substrate aging, metal conductivity and service life degradation).
[0005] Therefore, there is an urgent need to develop a method that is simple, environmentally friendly, energy-saving, highly controllable, and highly effective in doping carbon nanotubes, can form a carbon nanotube conductive path, and can effectively reduce the contact resistance in the device. Summary of the invention
[0006] In order to overcome the problems of poor effectiveness, poor repeatability, high cost, high pollution, and high contact resistance between carbon nanotubes and metal electrodes in small and medium-sized devices or electronic components in the prior art, the purpose of the present invention is to provide a nitrogen-doped carbon nanotube and a preparation method and application thereof.
[0007] The inventive concept of the present invention is: the present invention proposes a method for preparing nitrogen-doped carbon nanotubes, including preparing a low-concentration carbon nanotube dispersion; using a dielectric electrophoresis assembly method on a metal electrode with grooves to assemble a layer of carbon nanotube material on the groove portion to obtain a channel electrode after assembling carbon nanotubes; placing a nitrogen source next to the channel electrode after assembling carbon nanotubes and keeping a distance (the distance is 1cm to 5cm), heating the nitrogen source, and then applying a pulse voltage to the metal or alloy parts at both ends of the channel electrode after assembling carbon nanotubes, and obtaining nitrogen-doped metallic carbon nanotubes through local Joule heat doping (i.e., the process coupling of vapor deposition doping and local Joule heat). The method for preparing nitrogen-doped carbon nanotubes of the present invention can also be further provided with an additional step of electrical selective etching, so that nitrogen-doped semiconductor carbon nanotubes are finally obtained. The present invention not only realizes in-situ doping of carbon nanotubes on the device but also effectively improves the contact performance between the carbon nanotubes and metals (for example, improving the bonding performance of the contact between the two materials and reducing their contact resistance) through the process coupling and synergistic effect of vapor deposition doping and local Joule heat.
[0008] In short, the key to the present invention is to use local Joule heating method to replace the traditional high-temperature heat treatment and acid oxidation methods, perform pulse heating only at the contact position between the carbon nanotubes and the metal electrode, control the voltage and heating time, introduce functional groups and defect sites, activate the carbon nanotubes, and then dope the carbon nanotubes by evaporating the doping source and through vapor deposition, thereby improving its contact performance with the metal.
[0009] In order to achieve the above object, the technical solution adopted by the present invention is:
[0010] In a first aspect, the present invention provides a method for preparing nitrogen-doped carbon nanotubes, comprising the following steps:
[0011] 1) adding a carbon nanotube dispersion to the groove of the channel electrode and performing dielectrophoresis assembly to obtain a channel electrode assembled with carbon nanotubes;
[0012] 2) performing vapor deposition doping on the channel electrode assembled with the carbon nanotubes, and applying voltage to the channel electrode assembled with the carbon nanotubes during the vapor deposition doping process to obtain nitrogen-doped carbon nanotubes.
[0013] Preferably, in step 1), the width of the groove of the channel electrode is less than 50 μm.
[0014] Specifically, the method for preparing nitrogen-doped carbon nanotubes is suitable for processing or manufacturing micro-nano level devices.
[0015] Preferably, in step 1), the width of the groove of the channel electrode is 2 μm to 20 μm.
[0016] Further preferably, in step 1), the width of the groove of the channel electrode is 3 μm to 5 μm.
[0017] Preferably, the amount of the carbon nanotube dispersion in step 1) is 0.1uL to 10uL.
[0018] Further preferably, the amount of the carbon nanotube dispersion in step 1) is 0.5uL to 2uL.
[0019] Preferably, the concentration of the carbon nanotube dispersion in step 1) is 0.5 ug / mL to 10 ug / mL.
[0020] More preferably, the concentration of the carbon nanotube dispersion in step 1) is 1 ug / mL to 5 ug / mL.
[0021] Preferably, the continuous phase of the carbon nanotube dispersion in step 1) is one or more of N,N-dimethylformamide, ethylene glycol, glycerol, toluene, xylene, hexane, cyclohexane, dioxane, ethanol, acetone, ethylene glycol methyl ether acetate, and cyclohexanone.
[0022] Specifically, the continuous phase is volatile and can be easily removed, and N,N-dimethylformamide and the "dimethylformamide" in the examples are substantially the same substance.
[0023] Further preferably, the continuous phase of the carbon nanotube dispersion in step 1) is one or more of N,N-dimethylformamide, ethylene glycol, glycerol, ethanol, acetone, and cyclohexanone.
[0024] Preferably, the method for preparing the carbon nanotube dispersion in step 1) comprises the following steps:
[0025] The carbon nanotubes and the organic solvent are mixed and subjected to ultrasonic vibration to obtain a carbon nanotube suspension of 0.5 mg / mL to 10 mg / mL;
[0026] The carbon nanotube suspension of 0.5 mg / mL to 10 mg / mL is diluted with an organic solvent, ultrasonically shaken and centrifuged again, and the supernatant is collected and sealed for storage to obtain a carbon nanotube dispersion.
[0027] Preferably, the centrifugal force used in the centrifugation is 10000g to 15000g.
[0028] More preferably, the centrifugal force used in the centrifugation is 11000g to 13000g.
[0029] Specifically, the centrifugation in the method for preparing the carbon nanotube dispersion is to remove carbon nanotubes with larger sizes that cannot be dispersed.
[0030] Preferably, the supernatant accounts for 70% to 90% of the volume of the suspension after centrifugation.
[0031] Preferably, in step 1), the channel electrode comprises a substrate, a groove and a plurality of conductive patterns, the conductive patterns are fixed on the substrate, and a groove is provided between every two conductive patterns.
[0032] Specifically, the width of the groove is the distance between two conductive patterns.
[0033] Preferably, the material of the substrate is one or more of single crystal silicon, polycrystalline silicon, quartz, and silicon carbide.
[0034] Preferably, the material of the conductive pattern includes one or more of metals and alloys.
[0035] Further preferably, the material of the conductive pattern includes one or more of titanium, iron, copper, gold, platinum, silver, tin, aluminum, nickel, and chromium.
[0036] More preferably, the conductive pattern has a multi-layer structure, including a titanium metal layer and a gold metal layer from bottom to top.
[0037] Preferably, the specific steps of the dielectrophoresis assembly in step 1) are: applying an alternating current with a voltage amplitude of 2Vpp to 15Vpp and a frequency of 1MHz to 12MHz to the groove electrodes.
[0038] Further preferably, the specific steps of the dielectrophoresis assembly in step 1) are: applying a sinusoidal alternating current with a voltage amplitude of 5Vpp to 10Vpp and a frequency of 1MHz to 10MHz to the groove electrodes.
[0039] Preferably, the carbon nanotubes in step 1) are single-walled carbon nanotubes or multi-walled carbon nanotubes.
[0040] Preferably, the voltage in step 1) is obtained using a function generator.
[0041] Preferably, step 1) further comprises the steps of water washing, inert gas purging and drying.
[0042] In some embodiments of the present invention, step 1) further comprises the step of performing electrical breakdown using a DC voltage of 8V to 10V for 20 to 60s.
[0043] Specifically, the technical solutions of the present invention mainly include two kinds (see Figure 3 ), one is a scheme that does not include the use of a higher voltage to electrically selectively etch the trench electrode, and the other is a scheme that also includes the use of a higher voltage to electrically selectively etch the trench electrode; the technical solution of the present invention can control the type of nitrogen-doped carbon nanotubes ultimately obtained by adding an "electrically selective etching" step (the types of nitrogen-doped carbon nanotubes include nitrogen-doped metallic carbon nanotubes and semiconductor-type nitrogen-doped carbon nanotubes, specifically, the IV test curve of the nitrogen-doped metallic carbon nanotubes is closer to linear, while the IV test curve of the nitrogen-doped semiconductor-type carbon nanotubes is nonlinear).
[0044] Preferably, the doping source in step 2) is one or more of dicyandiamide, melamine and urea.
[0045] Further preferably, the doping source in step 2) is melamine.
[0046] Specifically, the local hot doping method of the present invention utilizes heteroatom doping to provide an electron donor or acceptor through a dopant, and after doping, the concentration of electron or hole carriers in the carbon nanotube increases, thereby enhancing its own conductivity. When the metallic carbon nanotube is in contact with the metal and then doped, the doping can increase the contact area between the carbon nanotube and the electrode, thereby improving its contact resistance; when the semiconductor carbon nanotube is in contact with the metal electrode, due to the difference in the Fermi energy levels of the two, there is a Schottky barrier and a local space electric field, and the doping can adjust the energy level distribution of the semiconductor carbon nanotube, reduce the barrier height of its contact with the metal, thereby improving the contact resistance.
[0047] Preferably, in step 2), the distance between the doping source and the channel electrode is 1 cm to 5 cm.
[0048] Preferably, the amount of the doping source in step 2) is 0.02 g to 0.5 g.
[0049] Further preferably, the amount of the doping source in step 2) is 0.04 g to 0.3 g.
[0050] Preferably, the heating in step 2) is specifically set to heat to 300° C. to 600° C. and maintain for 1 to 10 minutes.
[0051] Preferably, the voltage application in step 2) is carried out under the conditions of an absolute gas pressure of 0.01 Pa to 10 Pa and a temperature of 300° C. to 600° C.
[0052] Further preferably, the voltage application in step 2) is carried out under the conditions of an absolute gas pressure of 5Pa to 9Pa and a temperature of 400°C to 600°C.
[0053] Preferably, the voltage in step 2) is a pulsed square wave voltage with a voltage value of 1V to 8V and a frequency of 0.5 to 2kHz.
[0054] Further preferably, the voltage in step 2) is a pulsed square wave voltage with a voltage value of 5V to 7V and a frequency of 1kHz.
[0055] Specifically, the voltage selection range of the dielectric assembly is relatively large, and the voltage applied in the "Joule heat doping" step is recommended to be below 8V in order to avoid breakdown of the carbon nanotube pathway, thereby failing to achieve the technical effect of "effectively reducing contact resistance while maintaining a complete conductive pathway."
[0056] Preferably, the time for applying voltage in step 2) is 1 min to 2 min.
[0057] Specifically, step 2) is to place the channel electrode assembled with carbon nanotubes at a straight-line distance of 1 cm to 5 cm from the doping source, heat the doping source to a set temperature under a reduced pressure or vacuum environment, and apply a pulsed square wave to the conductive patterns at both ends of the channel electrode at the set temperature for 1 to 2 minutes, and then continue to maintain the doping source at the set temperature for vapor deposition to obtain nitrogen-doped carbon nanotubes.
[0058] Preferably, step 2) also includes the following steps:
[0059] Weigh the doping source, perform vapor deposition doping on the channel electrode assembled with carbon nanotubes, apply voltage to the channel electrode assembled with carbon nanotubes during the vapor deposition doping process, and repeat the above steps 1 to 6 times.
[0060] Preferably, the repetition number is 3 to 4 times.
[0061] In a second aspect, the present invention provides a nitrogen-doped carbon nanotube prepared by the method for preparing the nitrogen-doped carbon nanotube according to the first aspect.
[0062] Preferably, the contact resistance formed between the nitrogen-doped carbon nanotubes and the channel electrode is 0.1 MΩ to 4 MΩ.
[0063] Further preferably, the contact resistance formed between the nitrogen-doped carbon nanotubes and the channel electrode is 0.2 MΩ to 3.6 MΩ.
[0064] In a third aspect, the present invention provides an electronic device comprising the nitrogen-doped carbon nanotubes and conductive patterns described in the second aspect; the number of the conductive patterns is greater than 2, and the two conductive patterns are connected by the nitrogen-doped carbon nanotubes.
[0065] In a fourth aspect, the present invention provides a use of the nitrogen-doped carbon nanotubes in the manufacture of electronic devices or electronic components.
[0066] Preferably, the electronic device is a micro-nano device.
[0067] Specifically, the micro-nano device may be a flexible device, and the micro-nano device can be particularly applicable to the manufacture or processing of nanowires, flexible wires, conductive films and field effect transistors in the field of micro-nano electronics.
[0068] Preferably, the volume of the electronic device is less than 100 mm 3 .
[0069] Further preferably, the volume specification of the electronic device is less than 50mm 3 .
[0070] The beneficial effects of the present invention are as follows: the preparation method of nitrogen-doped carbon nanotubes in the present invention includes the steps of dielectrophoresis assembly and local Joule heat doping, which not only has the advantages of high preparation efficiency, good doping effect, simple preparation method, strong controllability, environmental protection, and suitable for the processing technology of small amount of carbon nanotubes and assembled electronic devices, but also has the effect of effectively reducing the contact resistance between carbon nanotubes and metals, and is particularly suitable for wire connection in micro-nano devices and flexible devices. Specifically:
[0071] (1) The method for preparing nitrogen-doped carbon nanotubes of the present invention not only has the advantages of low production cost, requiring less carbon nanotube raw material, and avoiding the need for acid treatment and the involvement of a large amount of organic solvents, but also is simple, fast and effective in doping, and can effectively reduce the contact resistance between the carbon nanotubes and the metal electrode and improve the contact performance (i.e., the bonding strength between the carbon nanotubes and the metal electrode);
[0072] (2) The method for preparing nitrogen-doped carbon nanotubes of the present invention is suitable for the manufacture and secondary processing of miniaturized electronic devices. It has little impact on the substrate and metal electrodes (or conductive patterns) on the device. It can not only improve the comprehensive contact performance between the carbon nanotubes and the metal electrodes to exert the excellent performance of the carbon nanotubes themselves, but also help to improve the service life of miniaturized electronic devices.
[0073] (3) The method for preparing nitrogen-doped carbon nanotubes of the present invention can make the contact resistance between the carbon nanotubes and the metal electrode reach 0.82MΩ to 3.6MΩ;
[0074] (4) Both the dielectrophoretic assembly and the local Joule heating in the method for preparing nitrogen-doped carbon nanotubes of the present invention require the application of voltage, which means that the method requires relatively few devices, has a high degree of matching between steps, is simpler in process operation, and has relatively good continuity between processes;
[0075] (5) The method for preparing carbon nanotubes of the present invention can be applied to the manufacture of micro-nano devices, and can be specifically used to form pathways on the devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1 It is a top view of the channel electrode in the present invention and a local enlarged view of the groove part of the channel electrode.
[0077] Figure 2 It is a physical schematic diagram of the channel electrode of the single crystal silicon substrate and the channel electrode of the quartz substrate in the present invention.
[0078] Figure 3 The figure is a flow chart of the preparation process of nitrogen-doped carbon nanotubes in the present invention.
[0079] Figure 4 This is a scanning electron microscope image of the groove portion of the channel electrode assembled by dielectric electrophoresis in Example 1.
[0080] Figure 5 This is a scanning electron microscope image of the groove portion of the channel electrode after local Joule heat doping in Example 1.
[0081] Figure 6 This is a diagram showing the IV test results of the channel electrode assembled by dielectric electrophoresis and the channel electrode after local Joule heat doping in Example 1.
[0082] Figure 7 This is a diagram showing the IV test results of the channel electrode after electrically selective etching and the channel electrode after local Joule heat doping in Example 2.
[0083] Figure 8 This is a diagram showing the IV test results of the channel electrode assembled by dielectric electrophoresis and the channel electrode after local Joule heat doping for different times in Example 3.
[0084] Fig. 9 This is a graph showing the IV test results of the channel electrode assembled by dielectric electrophoresis and the channel electrode doped by ordinary vapor deposition in Comparative Example 1.
[0085] Fig.10 This is a linear fitting result diagram of the IV curves of the channel electrode assembled by dielectric electrophoresis and the channel electrode after local Joule heat doping in Example 1. DETAILED DESCRIPTION
[0086] The present invention is further described in detail below through specific examples.
[0087] The "metallic SWCNT", "metallic carbon nanotube" or "metallic single-walled carbon nanotube" in the present invention refers to carbon nanotubes with good electrical conductivity; the conductive path assembled by using such carbon nanotubes mainly relies on the carbon nanotubes with low resistance to play a leading role, and its IV curve (see Figure 6 and Fig.10 ) meets the following characteristics:
[0088] (1) The overall IV curve has a high degree of linearity;
[0089] (2) There is no obvious "plateau" in the IV curve when it is close to 0V, and the Schottky barrier is small;
[0090] (3) As the voltage increases, not only does the value of the apparent resistance remain relatively constant, but the apparent resistance basically exhibits the characteristics of "Ohmic contact", thus presenting a linear or quasi-linear current-voltage characteristic.
[0091] The "semiconductor SWCNT", "semiconductor carbon nanotube" or "semiconductor single-walled carbon nanotube" in the present invention refers to carbon nanotubes with poor electrical conductivity; the IV curve of the conductive path assembled by using such carbon nanotubes (see Figure 7 ) meets the following characteristics:
[0092] (1) The overall IV curve is nonlinear; as the voltage increases, the apparent resistance basically shows the characteristics of a "Schottky contact";
[0093] (2) When approaching 0V, the IV curve shows an obvious "plateau", indicating that the Schottky barrier is large;
[0094] (3) As the voltage increases, not only does the apparent resistance of the conductive path become larger and more complex, but also a higher voltage is required to overcome the characteristics of the Schottky barrier.
[0095] A top view of the structure of the channel electrode used in the present invention and a local enlarged view of the groove portion of the channel electrode are shown in FIG. Figure 1 As shown, Figure 1 The size of the groove is for reference only and cannot be used as a basis for limiting its specific size. Figure 2 (a) in the figure; a schematic diagram of a channel electrode of a quartz substrate of the present invention, as shown in FIG. Figure 2 As shown in (b) in .
[0096] Depend on Figure 1It can be seen that: the channel electrode design of the present invention uses silicon material (for example, single crystal silicon, quartz, silicon polycrystalline, silicon carbide, etc.) as a substrate; two sheets of conductive metals or alloys (for example, platinum, gold, copper, titanium, silver and other metals and their alloys) are fixed on the surface of the substrate, and a groove is left between the two sheets of conductive metals or alloys; wherein the groove part is exposed to silicon material, and the spacing between the grooves is 3μm.
[0097] The volume of the channel electrode of the single crystal silicon substrate with a single channel electrode pattern is 4 mm × 7 mm × 2 mm (see Figure 2 (a)), the volume of the channel electrode of the quartz substrate with two channel electrode patterns is 5mm×8mm×2mm (see Figure 2 (b) in the figure.
[0098] Unless otherwise specified, the multiple electrodes with channel electrode patterns used in the embodiments and comparative examples are convenient for comparison between groups. Each channel electrode with a channel electrode pattern is based on a single crystal silicon substrate as a substrate, and the substrate surface has a conductive pattern, and a groove is provided between the two conductive patterns (the spacing between the grooves is 3 μm, and the material of the groove part is determined by the substrate, which is specifically a silicon material), and the conductive pattern is composed of a metal or alloy with good conductivity. The metal with good conductivity is titanium and gold from the bottom to the surface, and its structure is as follows: Figure 2 As shown; the rest of the raw materials are commercially available reagents or materials. Moreover, the silicon material of the substrate of the channel electrode used in the embodiment and the comparative example is only used as a substrate in the preparation of nitrogen-doped nanotubes, indicating that the preparation method thereof can be applied to the processing of semiconductor materials or sensors.
[0099] The process flow chart of the preparation of nitrogen-doped carbon nanotubes in the present invention is as follows: Figure 3 As shown. Figure 3 It can be seen that the preparation process of the nitrogen-doped carbon nanotubes of the present invention specifically involves a preparation process of local Joule heat doping, and its preparation process includes two parallel schemes.
[0100] The preparation process of the first scheme includes: preparing a carbon nanotube dispersion; using the dielectric electrophoresis assembly method on the metal electrode with grooves to assemble a layer of carbon nanotube material on the groove portion to obtain a channel electrode after assembling the carbon nanotubes; placing a nitrogen source next to the channel electrode after assembling the carbon nanotubes and maintaining a distance (the distance is 1cm to 5cm), heating the nitrogen source, and then applying a voltage to the metal or alloy parts at both ends of the channel electrode after assembling the carbon nanotubes, and obtaining nitrogen-doped metallic carbon nanotubes through local Joule heat doping.
[0101] The preparation process of the second scheme includes: preparing a carbon nanotube dispersion; using a dielectric electrophoresis assembly method on a metal electrode with grooves to assemble a layer of carbon nanotube material on the groove portion to obtain a channel electrode after assembling carbon nanotubes; applying voltage to the channel electrode after assembling carbon nanotubes to perform breakdown to obtain a channel electrode after electro-selective etching; placing a nitrogen source next to the channel electrode after electro-selective etching and keeping a distance (the distance is 1 cm to 5 cm), heating the nitrogen source, and then applying voltage to the metal or alloy parts at both ends of the channel electrode after electro-selective etching to obtain nitrogen-doped semiconductor carbon nanotubes through local Joule heat doping;
[0102] Among them, carbon nanotubes can be generally divided into semiconductor carbon nanotubes and metallic carbon nanotubes according to their conductivity. The "breakdown" of the second technical solution specifically utilizes the characteristic that "the resistance of semiconductor carbon nanotubes is greater than that of metallic carbon nanotubes". According to Q=U 2 ×t / R (Q is Joule heat, U represents the applied voltage, t represents the time of voltage application, and R represents resistance). Therefore, under the conditions of the same applied voltage and time, the Joule heat generated by metallic carbon nanotubes is greater than that of semiconductor tubes. As a result, metallic carbon nanotubes are more easily oxidized and burned out. Therefore, after the "breakdown" process, the carbon nanotubes on the substrate are theoretically all semiconductor carbon nanotubes.
[0103] The “applying voltage” or “applying power” in the embodiments and comparative examples of the present invention is achieved by connecting the power supply or voltage to the conductive metal electrodes at both ends of the channel electrode.
[0104] Example 1
[0105] This embodiment provides a method for preparing nitrogen-doped carbon nanotubes, comprising the following steps:
[0106] 1) Preparation of carbon nanotube dispersion: Weigh 1 mg of single-walled carbon nanotubes (SWCNTs) and put them into a 100 mL beaker. Use a measuring cylinder to measure 10 mL of dimethylformamide solvent (DMF), slowly pour it into the beaker containing the carbon nanotubes, and ultrasonically vibrate for 1 hour to obtain a 1 mg / mL carbon nanotube suspension.
[0107] Take 1 mL of 1 mg / mL carbon nanotube suspension and dilute it 100 times with dimethylformamide solvent, shake it again by ultrasonic vibration for 5 hours, and then centrifuge it at a centrifugal force of 12000g for 1 hour, take 90% (volume fraction) of the upper clear liquid, seal it and store it, and obtain 1 ug / mL carbon nanotube dispersion;
[0108] 2) Dielectrophoresis assembly: A channel electrode (size 4mm×7mm×2mm) with a single crystal silicon substrate and a channel spacing of 3μm was used, and 0.5uL of the carbon nanotube dispersion in step 1) was dripped onto the groove with a pipette, and the metal electrodes at both ends were connected to a function generator, and a sinusoidal alternating current with a voltage amplitude of 5Vpp and a frequency of 10MHz was applied for dielectrophoresis assembly. After applying the voltage for 3 minutes, the function generator was turned off, the dimethylformamide solvent was washed away with deionized water, and then the electrode surface was purged with nitrogen to remove the droplets on the surface, and then placed in a drying oven at 60°C for drying for 3 minutes to obtain a metallic single-walled carbon nanotube and a channel electrode assembled by dielectrophoresis;
[0109] 3) Local Joule heat doping: The channel electrode assembled by dielectrophoresis was placed at a linear distance of 2 cm from the doping source melamine (0.05 g), and the melamine was heated to 500 °C in a vacuum environment (absolute pressure of 8 Pa) for 5 min.
[0110] At the 3rd minute of heating, a pulsed square wave with a voltage of 6V and a frequency of 1kHz was applied to the metal patterns at both ends of the channel electrode for 1 minute, and vapor deposition was continued at 500°C for 2 minutes to obtain nitrogen-doped carbon nanotubes and a channel electrode after local Joule heat doping.
[0111] Wherein, g in step 1) is the acceleration due to gravity, and 12000g represents the magnitude of the centrifugal force;
[0112] The channel electrode assembled by dielectrophoresis in step 2) comprises a metallic single-walled carbon nanotube (metallic SWCNT) capable of forming a passage with the metal electrode;
[0113] The channel electrode after local Joule heat doping in step 3) contains nitrogen-doped metallic single-walled carbon nanotubes (metallic SWCNT doping) that can form a passage with the metal electrode.
[0114] Example 2
[0115] This embodiment provides a method for preparing nitrogen-doped carbon nanotubes. The difference between this embodiment and embodiment 1 is that this embodiment further includes an electrical selective etching step, specifically including the following steps:
[0116] 1) Preparation of carbon nanotube dispersion: Weigh 1 mg of single-walled carbon nanotubes (SWCNTs) and put them into a 100 mL beaker. Use a measuring cylinder to measure 10 mL of dimethylformamide solvent (DMF), slowly pour it into the beaker containing the carbon nanotubes, and ultrasonically vibrate for 1 hour to obtain a 1 mg / mL carbon nanotube suspension.
[0117] Take 1 mL of 1 mg / mL carbon nanotube suspension and dilute it 100 times with dimethylformamide solvent, shake it again by ultrasonic vibration for 5 hours, and then centrifuge it at a centrifugal force of 12000g for 1 hour, take 90% (volume fraction) of the upper clear liquid, seal it and store it, and obtain 1 ug / mL carbon nanotube dispersion;
[0118] 2) Dielectrophoresis assembly: A channel electrode (size 4mm×7mm×2mm) with a single crystal silicon substrate and a channel spacing of 3μm was used, and 0.5uL of the carbon nanotube dispersion in step 1) was dripped onto the groove using a pipette. The metal electrodes at both ends were connected to a function generator, and a sinusoidal alternating current with a voltage amplitude of 5Vpp and a frequency of 10MHz was applied for dielectrophoresis assembly. After applying the voltage for 3 minutes, the function generator was turned off, the dimethylformamide solvent was washed away with deionized water, and then the electrode surface was purged with nitrogen to remove the droplets on the surface, and then placed in a drying oven at 60°C for drying for 3 minutes to obtain a channel electrode assembled by dielectrophoresis;
[0119] 3) Electrically selective etching: The channel electrode assembled by dielectrophoresis was connected to a DC voltage source, the voltage was set to 8 V, and maintained for 30 seconds, and the channel electrode after electrical selective etching was obtained by electrical breakdown;
[0120] 4) Local Joule heat doping: The channel electrode after electro-selective etching was placed at a straight-line distance of 2 cm from the doping source melamine (0.05 g), and the melamine was heated to 500°C in a vacuum environment (absolute pressure of 8 Pa) for 5 min;
[0121] At the 3rd minute of heating, a pulsed square wave with a voltage of 6V and a frequency of 1kHz was applied to the metal patterns at both ends of the channel electrode for 1 minute to perform vapor deposition, thereby obtaining nitrogen-doped carbon nanotubes and channel electrodes after local Joule heat doping (i.e., electronic devices containing nitrogen-doped carbon nanotubes, denoted as semiconductor-type SWCNT doping);
[0122] Wherein, g in step 1) is the acceleration due to gravity, and 12000g represents the magnitude of the centrifugal force;
[0123] The channel electrode assembled by dielectrophoresis in step 2) comprises a metallic single-walled carbon nanotube (metallic SWCNT) capable of forming a passage with the metal electrode;
[0124] The channel electrode after the electrical selective etching in step 3) contains a semiconductor single-walled carbon nanotube (semiconductor SWCNT) that can form a path with the metal electrode.
[0125] The channel electrode after local Joule heat doping in step 4) contains semiconductor single-walled carbon nanotubes (semiconductor SWCNT doping) that can form a passage with the metal electrode.
[0126] Example 3
[0127] This embodiment provides a method for preparing nitrogen-doped carbon nanotubes. The difference between this embodiment and embodiment 1 is that the local Joule heat doping in this embodiment is performed multiple times, specifically including the following steps:
[0128] 1) Preparation of carbon nanotube dispersion: Weigh 1 mg of single-walled carbon nanotubes (SWCNTs) and put them into a 100 mL beaker. Use a measuring cylinder to measure 10 mL of dimethylformamide solvent (DMF), slowly pour it into the beaker containing the carbon nanotubes, and ultrasonically vibrate for 1 hour to obtain a 1 mg / mL carbon nanotube suspension.
[0129] Take 1 mL of 1 mg / mL carbon nanotube suspension and dilute it 100 times with dimethylformamide solvent, shake it again by ultrasonic vibration for 5 hours, and then centrifuge it at a centrifugal force of 12000g for 1 hour, take 90% (volume fraction) of the upper clear liquid, seal it and store it, and obtain 1 ug / mL carbon nanotube dispersion;
[0130] 2) Dielectrophoresis assembly: A channel electrode (size 4mm×7mm×2mm) with a single crystal silicon substrate and a channel spacing of 3μm was used, and 0.5uL of the carbon nanotube dispersion in step 1) was dripped onto the groove using a pipette. The metal electrodes at both ends were connected to a function generator, and a sinusoidal alternating current with a voltage amplitude of 5Vpp and a frequency of 10MHz was applied for dielectrophoresis assembly. After applying the voltage for 3 minutes, the function generator was turned off, the dimethylformamide solvent was washed away with deionized water, and then the electrode surface was purged with nitrogen to remove the droplets on the surface, and then placed in a drying oven at 60°C for drying for 3 minutes to obtain a channel electrode assembled by dielectrophoresis;
[0131] 3) Local Joule heat doping: The channel electrode assembled by dielectrophoresis was placed at a linear distance of 2 cm from the doping source melamine (0.05 g), and the melamine was heated to 500 °C in a vacuum environment (absolute pressure of 8 Pa) for 5 min.
[0132] At the 3rd minute of heating, a pulsed square wave with a voltage of 6V and a frequency of 1kHz was applied to the metal patterns at both ends of the channel electrode for 1 minute to perform vapor deposition;
[0133] Repeat the above steps of weighing 0.05 g of doping source melamine, placing the doping source at the same position, and applying the same pulse square wave under the same conditions to perform local Joule heat doping, to obtain nitrogen-doped carbon nanotubes with different doping times and channel electrodes after local Joule heat doping (i.e., electronic devices containing nitrogen-doped carbon nanotubes);
[0134] Wherein, g in step 1) is the acceleration due to gravity, and 12000g represents the magnitude of the centrifugal force;
[0135] The channel electrode assembled by dielectrophoresis in step 2) comprises a metallic single-walled carbon nanotube (SWCNT undoped) capable of forming a passage with the metal electrode;
[0136] The channel electrode after local Joule heat doping in step 3) contains metallic single-walled carbon nanotubes (metallic SWCNT doping) that can form a passage with the metal electrode;
[0137] The channel electrode after local Joule thermal doping obtained by performing local Joule thermal doping once in step 3) is recorded as SWCNT doping 1; the channel electrode after local Joule thermal doping obtained by performing local Joule thermal doping twice in step 3) is recorded as SWCNT doping 2; the channel electrode after local Joule thermal doping obtained by performing local Joule thermal doping three times in step 3) is recorded as SWCNT doping 3; the channel electrode after local Joule thermal doping obtained by performing local Joule thermal doping four times in step 3) is recorded as SWCNT doping 4.
[0138] Comparative Example 1
[0139] This comparative example provides a method for preparing nitrogen-doped carbon nanotubes. The difference from the other examples 1 is that no local Joule heat is introduced during the carbon nanotube doping process. Specifically, the method comprises the following steps:
[0140] 1) Preparation of carbon nanotube dispersion: Weigh 1 mg of single-walled carbon nanotubes (SWCNTs) and put them into a 100 mL beaker. Use a measuring cylinder to measure 10 mL of dimethylformamide solvent (DMF), slowly pour it into the beaker containing the carbon nanotubes, and ultrasonically vibrate for 1 hour to obtain a 1 mg / mL carbon nanotube suspension.
[0141] Take 1 mL of 1 mg / mL carbon nanotube suspension and dilute it 100 times with dimethylformamide solvent, shake it again by ultrasonic vibration for 5 hours, and then centrifuge it at a centrifugal force of 12000g for 1 hour, take 90% (volume fraction) of the upper clear liquid, seal it and store it, and obtain 1 ug / mL carbon nanotube dispersion;
[0142] 2) Dielectrophoresis assembly: A channel electrode (size 4mm×7mm×2mm) with a single crystal silicon substrate and a channel spacing of 3μm was used, and 0.5uL of the carbon nanotube dispersion in step 1) was dripped onto the groove using a pipette. The metal electrodes at both ends were connected to a function generator, and a sinusoidal alternating current with a voltage amplitude of 5Vpp and a frequency of 10MHz was applied for dielectrophoresis assembly. After applying the voltage for 3 minutes, the function generator was turned off, the dimethylformamide solvent was washed away with deionized water, and then the electrode surface was purged with nitrogen to remove the droplets on the surface, and then placed in a drying oven at 60°C for drying for 3 minutes to obtain a channel electrode assembled by dielectrophoresis;
[0143] 3) Ordinary vapor deposition doping: The channel electrode assembled by dielectrophoresis was placed at a straight-line distance of 2 cm from 0.05 g of melamine, and the melamine was heated to 500° C. and maintained for 5 min under a vacuum environment (absolute pressure of 8 Pa) for vapor deposition to obtain ordinary nitrogen-doped carbon nanotubes and channel electrodes doped by ordinary vapor deposition;
[0144] Wherein, g in step 1) is the acceleration due to gravity, and 12000g represents the magnitude of the centrifugal force;
[0145] The channel electrode assembled by dielectrophoresis in step 2) comprises a metallic single-walled carbon nanotube (SWCNT undoped) capable of forming a passage with the metal electrode;
[0146] The channel electrode after conventional vapor deposition doping in step 3) contains nitrogen-doped carbon nanotubes (SWCNT conventional vapor deposition doping) that can form a passage with the metal electrode.
[0147] Performance Testing
[0148] 1. The scanning electron microscope image of the groove portion of the channel electrode assembled by dielectric electrophoresis in Example 1 is as follows: Figure 4 The scanning electron microscope image of the groove portion of the channel electrode after local Joule heat doping in Example 1 is shown in FIG. Figure 5 shown.
[0149] Depend on Figure 4 and Figure 5 It can be seen that the brighter parts at both ends of the SEM image are metal electrodes, and the middle part is the groove. Figure 4 A continuous path composed of carbon nanotubes can be observed, indicating that a carbon nanotube layer can be firmly formed on the groove surface after dielectrophoresis assembly, and the carbon nanotubes on the carbon nanotube layer can build a connected path for the metal electrodes on both sides under the action of dielectrophoresis. Figure 4In comparison, the nitrogen-doped carbon nanotube layer on the groove surface of the composite electrode containing nitrogen-doped carbon nanotubes obtained after local Joule heat doping has a smoother appearance, the distribution of nitrogen-doped carbon nanotubes is more dispersed and uniform, and the combination with the metal electrodes at both ends is more firmly established, which is beneficial to the connectivity between the groove part and the metal parts at both ends, and thus creates conditions for reducing the contact potential to a certain extent.
[0150] 2. Under the conditions of temperature of 25°C, voltage of 0-2.5V, and step of 0.1V, the carbon nanotubes assembled between the channel electrodes in the embodiment and the comparative example were tested by touching the square metal patterns at both ends with the probes on the source meter before and after doping, and the resistance was calculated based on the voltage 2V data on the IV curve; the relevant IV test results are shown in FIG. Figure 6 to Figure 9 shown.
[0151] The apparent resistance measured by the test method of the present invention is composed of metal resistance, carbon nanotube resistance and contact resistance. In this field, in order to study the contact resistance between metal and carbon nanotube, the technicians in this field usually ignore the smaller resistance of metal and carbon nanotube, and think that the measured apparent resistance is approximately equal to the contact resistance. Since the resistance of carbon nanotube and metal are relatively small, especially the resistance of gold and titanium metal, and the conductive path on the channel electrode is only built by single-walled carbon nanotube, the VI curve and the measured apparent resistance can reflect the characteristics of carbon nanotube on the conductive path after assembly and doping, and the relative size of the contact resistance on the path assembled by metal and carbon nanotube to a certain extent.
[0152] The IV test results of the channel electrode assembled by dielectric electrophoresis and the channel electrode after local Joule heat doping in Example 1 are shown in FIG. Figure 6 The original current and voltage data in the IV curve test of the channel electrode assembled by dielectric electrophoresis and the channel electrode after local Joule heat doping in Example 1 were linearly fitted, and the fitting results are shown in FIG. Fig.10 shown.
[0153] Depend on Figure 6 and Fig.10It can be seen that: the test results with a selected voltage of 2V are calculated and analyzed, and the apparent resistance of the channel electrode after dielectrophoresis assembly is calculated to be 10.33MΩ, while the apparent resistance of the channel electrode after local Joule heat doping is 3.59MΩ. Since the apparent resistances are all greater than 1MΩ, it can be explained that the apparent resistance is mainly the contact resistance between the metal and the carbon nanotube. Comparing the apparent resistance between the carbon nanotube and the metal, under the same test voltage (2V), the current flowing through the channel electrode after local Joule heat doping is higher, and the apparent resistance decreases by 65.2%, indicating that this method can not only produce nitrogen-doped carbon nanotubes, but also be suitable for doping and modification of assembled metal-type carbon nanotube devices, thereby improving the contact performance of carbon nanotubes and metals (improving their firmness), and reducing the contact resistance of electrodes or electronic devices, thereby creating conditions for improving the safety of electrodes or electronic devices and reducing unnecessary energy consumption.
[0154] At the same time, for the IV test raw data of the channel electrode assembled by dielectrophoresis in Example 1, the equation obtained by software fitting is: y=0.0988x+0.0153, and its correlation coefficient R 2 =0.9834; and for the original data of the IV test of the channel electrode after local Joule heat doping in Example 1, the equation obtained by software fitting is: y=0.2828x-0.0153, and its correlation coefficient R 2 =0.9969. The R of the fitting curve results of the channel electrode assembled by dielectrophoresis and the channel electrode after local Joule heat doping in Example 1 is 2 ≥0.9, indicating that the linearity of the overall IV curve is relatively high, which is approximately equivalent to "Ohmic contact". It can be judged that the two channel electrodes are basically pathways assembled by metallic single-walled carbon nanotubes, so they can be recorded as metallic SWCNT and metallic SWCNT doped, respectively.
[0155] Judging from the larger slope of the fitting curve of the metallic SWCNT, the overall apparent resistance of the channel electrode after local Joule heat doping is lower, which can explain that the local Joule doping method can not only better maintain the stability of the pathway assembled by carbon nanotubes, but also effectively reduce the contact resistance between carbon nanotubes and metals.
[0156] Using the same test method as above, the channel electrode after the electrical selective etching and the channel electrode after the local Joule heat doping in Example 2 were tested by a source meter. The test results are as follows: Figure 7 shown.
[0157] Depend on Figure 7It can be seen that the IV curves of the channel electrode after electro-selective etching (i.e., semiconductor SWCNT) and the channel electrode after local Joule heat doping (i.e., semiconductor SWCNT doping) in Example 2 are both nonlinear, and it can be determined that they are semiconductor carbon nanotubes; after local Joule heat doping, carriers are introduced into the semiconductor carbon nanotubes, the Fermi level in the energy band structure is adjusted, and the contact barrier between the carbon nanotubes and the metal electrode is reduced. Specifically, when the test voltage is 1.0 to 1.5 V, as the voltage increases, the current value of the semiconductor SWCNT doping first overcomes the contact barrier, the current first breaks through 0 A, and shows a faster upward trend (see Figure 6 ); when the test voltage is 1.0-2.5V, under the same test voltage, the current value of the semiconductor SWCNT doping is higher than that of the semiconductor SWCNT, indicating that this method is not only applicable to the assembled semiconductor carbon nanotube devices for nitrogen doping modification, but also can improve the contact performance between carbon nanotubes and metals, and reduce the contact resistance between carbon nanotubes and metals.
[0158] Using the same test method as above, IV tests were performed on the channel electrodes assembled by dielectric electrophoresis and the channel electrodes after local Joule heat doping for different times in Example 3 using a source meter. The test results are as follows: Figure 8 As shown; the composite electrode of nitrogen-doped carbon nanotubes obtained by local Joule heat doping once in Example 3 is recorded as SWCNT-doping 1; the composite electrode of nitrogen-doped carbon nanotubes obtained by local Joule heat doping twice in Example 3 is recorded as SWCNT-doping 2; and by analogy, the composite electrodes obtained by local Joule heat doping three and four times in Example 3 are recorded as SWCNT-doping 3 and SWCNT-doping 4.
[0159] Depend on Figure 8 It can be seen that: in Example 3, the channel electrode assembled by dielectric electrophoresis and the channel electrode after local Joule heat doping for different times were tested by source meter. The linearity of the IV curves of the carbon nanotubes before and after doping in Example 3 is good, and it can be judged that they are all metallic carbon nanotubes. The apparent resistance value of the carbon nanotubes before doping is 10.83MΩ; after analysis, the apparent resistance values of the channel electrodes after local Joule heat doping for 1, 2, 3 and 4 times are 2.90MΩ, 1.57MΩ, 1.10MΩ and 0.82MΩ, respectively, and the apparent resistance decreased by 73.2%, 45.9%, 29.9% and 25.5%, respectively (the comparison benchmark is the previous apparent resistance), which shows that with the increase of the number of local Joule heat doping, the decrease rate of contact resistance gradually decreases, indicating that the number of local Joule heat doping about 1 to 4 times has a relatively obvious effect on reducing the contact resistance between metal and carbon nanotubes.
[0160] At the same time, the above results also show that this method is not only applicable to multiple doping modifications of assembled carbon nanotube devices, but also that as the number of doping times increases, the contact performance between the carbon nanotubes and metals is improved, the apparent resistance is smaller, and the corresponding contact resistance is smaller.
[0161] Using the same test method as above, the undoped channel electrode (i.e., SWCNT undoped) and the channel electrode doped by conventional vapor deposition (i.e., SWCNT conventional vapor deposition doped) in Comparative Example 1 were tested by a source meter. The results of the IV test are shown in FIG. Fig. 9 shown.
[0162] Depend on Fig. 9 It can be seen that: the IV curve of the channel electrode before doping in Comparative Example 1 shows good linearity, which can be judged as a metallic carbon nanotube, with an apparent resistance of 7.46 MΩ; under the same voltage, the current of the channel electrode after ordinary vapor deposition nitrogen doping is higher, and the apparent resistance is 6.91 MΩ, and the apparent resistance has only decreased by 7.3%, indicating that its contact resistance has also decreased less. This is because the intrinsic carbon nanotubes have high stability and fewer defects. It is difficult to effectively dope and modify them without introducing defects through local Joule heat, thereby making it difficult to effectively reduce the contact resistance between metal and carbon nanotubes, which in turn leads to a certain degree of limitation in the application of doped carbon nanotubes in the manufacture of electronic components or electronic devices.
[0163] It should be noted that the main technical problems solved by the present invention include at least: reducing the contact resistance between carbon nanotubes and metal electrodes in miniaturized devices, and improving the contact performance between carbon nanotubes and metal electrodes. Although there is a certain deviation in the channel electrodes assembled by dielectrophoresis in the comparative example and the embodiment according to the IV curve test (due to the deviation in the number of pathways assembled by carbon nanotubes), it does not affect the technical solution of the present invention to solve its main technical problems.
[0164] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing nitrogen-doped carbon nanotubes, It is characterized in that The following steps are involved: 1) adding a carbon nanotube dispersion to the groove of the channel electrode and performing dielectrophoresis assembly to obtain a channel electrode assembled with carbon nanotubes; 2) performing vapor deposition doping on the channel electrode assembled with the carbon nanotubes, and applying voltage to the channel electrode assembled with the carbon nanotubes during the vapor deposition doping process to obtain nitrogen-doped carbon nanotubes; Step 1) The specific steps of the dielectrophoresis assembly are: applying an alternating current with a voltage amplitude of 2Vpp~15Vpp and a frequency of 1MHz~12MHz to the groove electrode; The step 1) further comprises the step of performing electrical breakdown using a DC voltage of 8V to 10V for 20 to 60s; The doping source used in step 2) is one or more of dicyandiamide, melamine, and urea; the voltage in step 2) is a pulsed square wave voltage with a voltage value of 1V to 8V and a frequency of 0.5kHz to 2kHz.
2. The method for preparing nitrogen-doped carbon nanotubes according to claim 1, Features: Step 1) The channel electrode comprises a substrate, a groove and a plurality of conductive patterns, wherein the conductive patterns are fixed on the substrate and a groove is provided between every two conductive patterns; the material of the conductive patterns comprises one or more of metals and alloys.
3. The method for preparing nitrogen-doped carbon nanotubes according to claim 1 or 2, Features: The amount of the carbon nanotube dispersion in step 1) is 0.1 μL to 10 μL; the concentration of the carbon nanotube dispersion in step 1) is 0.5 μg / mL to 10 μg / mL.
4. The method for preparing nitrogen-doped carbon nanotubes according to claim 1, Features: Step 2) also includes the following steps: Weigh the doping source, perform vapor deposition doping on the channel electrode assembled with the carbon nanotubes, apply voltage to the channel electrode assembled with the carbon nanotubes during the vapor deposition doping process, and repeat the above steps 1 to 6 times. 5 . Nitrogen-doped carbon nanotubes prepared by the method for preparing nitrogen-doped carbon nanotubes according to any one of claims 1 to 4 .
6. An electronic device, It is characterized in that The electronic device comprises the nitrogen-doped carbon nanotubes and conductive patterns as claimed in claim 5; the number of the conductive patterns is greater than 2, and the two conductive patterns are connected by the nitrogen-doped carbon nanotubes.
7. Use of the nitrogen-doped carbon nanotubes according to claim 5 in the manufacture of electronic devices or electronic components.