A microwave radiation technology to synthesize Mg 3 (OH) 4 (NO 3 ) 2 Materials and Methods

Synthesize Mg3(OH)4(NO3)2 ultra-thin nanosheet materials through microwave radiation technology, solving the problems of high energy consumption and difficult morphology regulation in the existing technology, and achieving high-quality and uniform morphology preparation of nanosheet materials , suitable for the development of multifunctional nanomaterials.

CN116143151BActive Publication Date: 2024-11-08SUZHOU UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310037886.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-07
Publication Date
2024-11-08
Estimated Expiration
2043-01-07

AI Technical Summary

Technical Problem

The prior art has problems such as high energy consumption, complex operation and difficulty in accurately regulating the micromorphology of the material when synthesizing Mg3(OH)4(NO3)2 ultra-thin nanosheet materials, which affects its application in the field of multifunctional nanomaterials.

Method used

Mg3(OH)4(NO3)2 material was synthesized by microwave radiation technology. By adjusting the reaction time, temperature and raw material molar ratio, sodium dodecylbenzenesulfonate SDBS was used as a surfactant, combining high-purity water and analyzing pure Mg(NO3 )2·6H2O and NaOH are used as raw materials to achieve high-quality and uniform morphology preparation of nanosheet materials.

Benefits of technology

It has achieved the preparation of high-purity, uniform morphology, and ultra-thin nanosheet materials with low energy consumption and simple operation. It has good dispersion and size control, and is suitable for anion exchangers and multifunctional Material development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116143151B_ABST
    Figure CN116143151B_ABST
Patent Text Reader

Abstract

A method for regulating the structure of Mg3(OH)4(NO3)2 ultra-thin nanosheet material by microwave radiation technology, using analytical pure Mg(NO3)2·6H2O and NaOH as reaction raw materials, high-purity water as solvent, sodium dodecylbenzene sulfonate SDBS as surfactant, and synthesizing Mg3(OH)4(NO3)2 material by microwave radiation technology. The characteristics of the microwave radiation method used in the process of synthesizing the target product Mg3(OH)4(NO3)2 material of the present invention are: the strong energy beam provided by the microwave radiation method makes the reaction solution heat more evenly, which is conducive to the synthesis of high-quality products, and the whole process of preparing the material is green and environmentally friendly, and no harmful substances are produced. The XRD diagram and SEM diagram of the product fully prove that the Mg3(OH)4(NO3)2 material synthesized by the microwave radiation method used in this patent has uniform morphology, small size and good dispersion; the target product Mg3(OH)4(NO3)2 material of the present invention can achieve functional diversification through ion exchange reaction.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] [Technical field]: The target product of the patent of this invention is mainly used in anion exchangers, and particularly relates to a method for regulating the structure of Mg3(OH)4(NO3)2 ultra-thin nanosheet materials using microwave radiation technology.

[0002] [Technical Background]: Layered Hydroxide Salts (LHSs) are favored by researchers because of their good chemical stability, biocompatibility and green environmental protection, as well as the large number of accessible active sites on the surface and the ability to undergo ion exchange reactions. LHSs have shown excellent performance in electrochemistry, photodegradation, sensors, energy storage materials and other fields (Sergio R. Tavares, Pedro Ivo R. Moraes, Rodrigo B. Capaz, et al. Novel 2D materials from exfoliation of layered hydroxide salts: A theoretical study [J]. Applied Surface Science. 2019, 483: 762-771).

[0003] Mg3(OH)4(NO3)2 is a relatively less studied layered hydroxide salt. In the Mg3(OH)4(NO3)2 structure, each layer consists of an octahedral cation (Mg 2+ ) and hydroxide anion (OH - ) coordination structure, one quarter of the octahedral sites are empty, surrounded by magnesium tetrahedra above and below: these magnesium tetrahedra share hydroxide ions with the octahedrons, while nitrate ions (NO3 -) is located between the layers to maintain charge balance. (Bin Liu. One-dimensional copper hydroxide nitrate nanorods and nanobelts for radiochemical applications [J]. Nanoscale. 2012, 4 (22): 7194-7198). There are many methods for synthesizing layered hydroxide salts, such as chemical precipitation, water / solvothermal method, electrodeposition, molten salt method, etc. (Guodong Xia and Sumei Wang. Microwave-assisted facile and rapid synthesis of layered metal hydroxide nanosheet arrays towards high-performance aqueous hybrid supercapacitors [J]. Ceramics International. 2019, 45 (16): 20810-20817; Sambandam Anandan, Jerry J. Wu and Muthupandian Ashokkumar. Sonochemical Synthesis of Layered Copper Hydroxy Nitrate Nanosheets [J]. Chem Phys Chem. 2015, 16 (16): 3389-3391). The target product Mg3(OH)4(NO3)2 material can be modified through anion exchange reaction to form a large number of multifunctional nanomaterials. The synthesis process is green and environmentally friendly, and no harmful substances are produced. It has potential research and application value.

[0004] A method for regulating the structure of Mg3(OH)4(NO3)2 ultrathin nanosheet material by microwave radiation technology, wherein analytically pure Mg(NO3)2·6H2O and NaOH are used as reaction raw materials, high-purity water is used as solvent, and sodium dodecylbenzene sulfonate SDBS is used as surfactant, and the Mg3(OH)4(NO3)2 material is synthesized by microwave radiation technology. Microwave radiation technology has low energy consumption and simple operation. The microscopic morphology of the target product can be precisely controlled by adjusting experimental conditions such as reaction time, reaction temperature, and raw material molar ratio, thereby obtaining high-quality Mg3(OH)4(NO3)2 material. The X-ray diffraction pattern (XRD pattern) of the obtained Mg3(OH)4(NO3)2 sample shows good agreement with the peaks of the standard card JCPDS No.26-1221, and there are no impurity peaks; from the scanning electron microscope image (SEM image) of the product, it can be concluded that the dispersion is good and the particle size range is narrow. The XRD and SEM images fully prove that the microwave radiation technology involved in the patent of this invention can synthesize Mg3(OH)4(NO3)2 materials with high purity and uniform morphology, which has distinct scientificity, practicality and novelty, and is widely used in the development of anion exchangers, multifunctional materials and other fields.

[0005]

Invention Content

[0006] [Technical solution of the present invention]: A method for regulating the structure of Mg3(OH)4(NO3)2 ultra-thin nanosheet material using microwave radiation technology, using analytical pure Mg(NO3)2·6H2O and NaOH as reaction raw materials, high-purity water as solvent, sodium dodecylbenzene sulfonate SDBS as surfactant, and synthesizing Mg3(OH)4(NO3)2 material using microwave radiation technology. The specific synthesis steps are as follows:

[0007] First, at room temperature, weigh 0.0100-10.0000 g of analytical pure Mg(NO3)2·6H2O, place it in a 100 mL beaker, add 1-70 mL of high-purity water, stir uniformly with a glass rod for 1-15 min, place the solution on a magnetic stirrer, and stir uniformly at a speed of 200-800 rpm for 0.5-2 h to obtain solution A;

[0008] Second, weigh 0.0100-60.0000 g of sodium dodecylbenzene sulfonate SDBS, transfer it to a beaker containing 1-100 mL of 0.1-5.0 mol / L NaOH, stir the solution uniformly with a glass rod for 1-15 min, place the solution on a magnetic stirrer, and stir at a speed of 200-800 rpm for 0.5-2 h to obtain a mixed solution B;

[0009] Third, the solution A obtained in the first step is transferred to a 250 mL quartz round-bottom flask, and the mixed solution B obtained in the second step is uniformly added dropwise to the 250 mL quartz round-bottom flask containing the solution A at a rate of 0.0050 to 10.0000 mL / min; after the dropwise addition is completed, the quartz round-bottom flask containing the reaction solution is placed on a magnetic stirrer and uniformly stirred at a speed of 200 to 800 rpm for 0.5 to 2 h to obtain a mixed solution C;

[0010] Fourth, the mixed solution C obtained in the third step is transferred to a modified PJ21C-AU Midea microwave reactor, which is equipped with a normal pressure reflux cooling device, a power of 200-1400 W, and a frequency of 2450 MHz; the reaction temperature is set to 80-100° C., and the reaction time is 0.1-5.0 h;

[0011] Fifth, after the reaction is completed, wait for the product in the quartz round-bottom flask to cool to room temperature, transfer the product to a centrifuge, centrifuge at a speed of 6000-10000 rpm for 1-5 minutes, pour off the supernatant, retain the lower layer product, and then wash the lower layer product with high-purity water and ethanol for 3-5 times; then place the obtained solid product in a forced air drying oven, adjust the heating rate to 5°C / min, and dry it in a forced air drying oven at 50-80°C for 5-24 hours to obtain the target Mg3(OH)4(NO3)2 material; the corresponding card number of the X-ray diffraction is 26-1221, and the crystal plane index corresponding to the strongest peak is (100); the product belongs to the orthorhombic system, and the unit cell parameter is α=β=γ=90.0°; the microstructure measured by field emission scanning electron microscope (SEM) at different magnifications is an ultra-thin nanosheet with a thickness of 60 to 100 nm and a diameter of 200 to 300 nm; this inorganic material is widely used in the fields of anion exchangers, multifunctional material development, etc.

[0012] [Advantages and effects of the invention]: A method for regulating the structure of Mg3(OH)4(NO3)2 ultra-thin nanosheet materials by microwave radiation technology, the advantages of which are: (1) Mg3(OH)4(NO3)2 is a typical magnesium-based layered hydroxide salt, which can form a large amount of functional materials through anion exchange reaction and has potential application value in various fields; (2) The microwave radiation technology involved in the patent of the present invention has low energy consumption and simple operation, and can eliminate the temperature difference between the inside and outside of the reaction raw materials, thereby improving the quality of the target product; (3) The microwave radiation method involved in the patent of the present invention can prepare a target product with uniform morphology, small size, good dispersion and high quality, which is the basis for Mg3(OH)4(NO3)2 material to exert its good performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 X-ray diffraction (XRD) crystallographic data of Mg3(OH)4(NO3)2c sample

[0014] Figure 2 The vertical a-axis observation results of the crystal structure of Mg3(OH)4(NO3)2 sample

[0015] Figure 3 The vertical b-axis observation results in the crystal structure of Mg3(OH)4(NO3)2 sample

[0016] Figure 4 The vertical c-axis observation results in the crystal structure of Mg3(OH)4(NO3)2 sample DETAILED DESCRIPTION

[0017] The following is a further description of the implementation and effects of the present invention in conjunction with the embodiments:

[0018] Example 1 Synthesis of Mg3(OH)4(NO3)2 Sample 1 using microwave radiation technology

[0019] At room temperature, weigh 3.9840 g of analytical pure Mg(NO3)2·6H2O, place it in a 100 mL beaker, add 50 mL of high-purity water, stir uniformly with a glass rod for 10 min, place the solution on a magnetic stirrer, and stir uniformly at 600 rpm for 1 h to obtain solution A; secondly, weigh 15.0000 g of sodium dodecylbenzene sulfonate SDBS, transfer it to 50 mL of 1.0 mol / L The mixture was placed in a beaker containing NaOH, stirred at a constant speed for 10 min with a glass rod, and then placed on a magnetic stirrer and stirred at a constant speed of 600 rpm for 1 h to obtain a mixed solution B; solution A was transferred to a 250 mL quartz round-bottom flask, and the mixed solution B was uniformly added dropwise to the 250 mL quartz round-bottom flask containing solution A at a rate of 2.0000 mL / min; after the addition was completed, the quartz round-bottom flask containing the reaction solution was placed on a magnetic stirrer and stirred at a constant speed of 600 rpm for 1 h to obtain a mixed solution C; the mixed solution C was then transferred to a modified PJ21C-AU Midea microwave reactor, which was equipped with a normal pressure reflux cooling device and a power of 1000W, frequency 2450MHz; set the reaction temperature to 100℃, reaction time to 1.0h; after the reaction is completed, wait for the product in the quartz round-bottom flask to cool to room temperature, transfer the product to a centrifuge, centrifuge at 8000rpm for 2min, pour out the supernatant, retain the lower layer product, and then wash the lower layer product with high-purity water and ethanol for 3 times; then place the obtained solid product in a forced air drying oven, adjust the heating rate to 5℃ / min, and dry it in a forced air drying oven at 60℃ for 20h to obtain the target Mg3(OH)4(NO3)2 material; the corresponding card number of the X-ray diffraction is 26-1221, and the crystal plane index corresponding to the strongest peak is (100)( Figure 1 ); the product belongs to the orthorhombic system ( Figures 2 to 4 ), the unit cell parameters are α=β=γ=90.0°; the microstructure measured by field emission scanning electron microscope (SEM) at different magnifications is an ultra-thin nanosheet with a thickness of 60 to 100 nm and a diameter of 200 to 300 nm; this inorganic material is widely used in the fields of anion exchangers, multifunctional material development, etc.

[0020] Example 2 Synthesis of Mg3(OH)4(NO3)2 Sample 2 using microwave radiation technology

[0021] At room temperature, 4.2901 g of analytical pure Mg(NO3)2·6H2O was weighed and placed in a 100 mL beaker. 50 mL of high-purity water was added. After stirring at a constant speed for 10 min with a glass rod, the solution was placed on a magnetic stirrer and stirred at a constant speed of 600 rpm for 1 h to obtain solution A. Next, 18.0000 g of sodium dodecylbenzene sulfonate SDBS was weighed and transferred to a 50 mL beaker containing 1.0 mol / L The mixture was placed in a beaker containing NaOH, stirred at a constant speed for 10 min with a glass rod, and then placed on a magnetic stirrer, and stirred at a constant speed of 600 rpm for 1 h to obtain a mixed solution B; solution A was transferred to a 250 mL quartz round-bottom flask, and the mixed solution B was uniformly added dropwise to the 250 mL quartz round-bottom flask containing solution A at a rate of 2.0000 mL / min; after the dropwise addition was completed, the quartz round-bottom flask containing the reaction solution was placed on a magnetic stirrer, and stirred at a constant speed of 600 rpm for 1 h to obtain a mixed solution C; the mixed solution C was then transferred to a modified PJ21C-AU Midea microwave reactor, and the microwave The wave reactor is equipped with a normal pressure reflux cooling device with a power of 1000W and a frequency of 2450MHz; the reaction temperature is set to 100℃ and the reaction time is 1.0h; after the reaction is completed, the product in the quartz round-bottom flask is cooled to room temperature, and the product is transferred to a centrifuge and centrifuged at 8000rpm for 2min, the supernatant is poured out, the lower layer product is retained, and the lower layer product is washed 3 times with high-purity water and ethanol; the solid product is then placed in a forced air drying oven, the heating rate is adjusted to 5℃ / min, and the target Mg3(OH)4(NO3)2 material is obtained after drying in a forced air drying oven at 60℃ for 20h.

[0022] Example 3 Synthesis of Mg3(OH)4(NO3)2 Sample 3 using microwave radiation technology

[0023] At room temperature, weigh 5.2017 g of analytical pure Mg(NO3)2·6H2O, place it in a 100 mL beaker, add 50 mL of high-purity water, stir uniformly with a glass rod for 10 min, place the solution on a magnetic stirrer, and stir uniformly at 600 rpm for 1 h to obtain solution A; secondly, weigh 20.0000 g of sodium dodecylbenzene sulfonate SDBS, transfer it to 50 mL of 1.0 mol / L The mixture was placed in a beaker containing NaOH, stirred at a constant speed for 10 min with a glass rod, and then placed on a magnetic stirrer, and stirred at a constant speed of 600 rpm for 1 h to obtain a mixed solution B; solution A was transferred to a 250 mL quartz round-bottom flask, and the mixed solution B was uniformly added dropwise to the 250 mL quartz round-bottom flask containing solution A at a rate of 2.0000 mL / min; after the dropwise addition was completed, the quartz round-bottom flask containing the reaction solution was placed on a magnetic stirrer, and stirred at a constant speed of 600 rpm for 1 h to obtain a mixed solution C; the mixed solution C was then transferred to a modified PJ21C-AU Midea microwave reactor, and the microwave The wave reactor is equipped with a normal pressure reflux cooling device with a power of 1000W and a frequency of 2450MHz; the reaction temperature is set to 100℃ and the reaction time is 1.0h; after the reaction is completed, the product in the quartz round-bottom flask is cooled to room temperature, and the product is transferred to a centrifuge and centrifuged at 8000rpm for 2min, the supernatant is poured out, the lower layer product is retained, and the lower layer product is washed 3 times with high-purity water and ethanol; the solid product is then placed in a forced air drying oven, the heating rate is adjusted to 5℃ / min, and the target Mg3(OH)4(NO3)2 material is obtained after drying in a forced air drying oven at 60℃ for 20h.

Claims

1. A method for regulating the structure of Mg3(OH)4(NO3)2 ultra-thin nanosheet material by microwave radiation technology, using analytical pure Mg(NO3)2·6H2O and NaOH as reaction raw materials, high-purity water as solvent, sodium dodecylbenzene sulfonate SDBS as surfactant, and synthesizing Mg3(OH)4(NO3)2 material by microwave radiation technology. The specific synthesis steps are as follows: First, at room temperature, weigh 0.0100-10.0000 g of analytical pure Mg(NO3)2·6H2O, place it in a 100 mL beaker, add 1-70 mL of high-purity water, stir uniformly with a glass rod for 1-15 min, place the solution on a magnetic stirrer, and stir uniformly at a speed of 200-800 rpm for 0.5-2 h to obtain solution A; Second, weigh 0.0100-60.0000 g of sodium dodecylbenzene sulfonate SDBS, transfer it to a beaker containing 1-100 mL of 0.1-5.0 mol / L NaOH, stir the solution uniformly with a glass rod for 1-15 min, place the solution on a magnetic stirrer, and stir at a speed of 200-800 rpm for 0.5-2 h to obtain a mixed solution B; Third, the solution A obtained in the first step is transferred to a 250 mL quartz round-bottom flask, and the mixed solution B obtained in the second step is uniformly added dropwise to the 250 mL quartz round-bottom flask containing the solution A at a rate of 0.0050 to 10.0000 mL / min; after the dropwise addition is completed, the quartz round-bottom flask containing the reaction solution is placed on a magnetic stirrer and uniformly stirred at a speed of 200 to 800 rpm for 0.5 to 2 h to obtain a mixed solution C; Fourth, the mixed solution C obtained in the third step is transferred to a modified PJ21C-AU Midea microwave reactor, which is equipped with a normal pressure reflux cooling device, a power of 200-1400 W, and a frequency of 2450 MHz; the reaction temperature is set to 80-100° C., and the reaction time is 0.1-5.0 h; Fifth, after the reaction is completed, wait for the product in the quartz round-bottom flask to cool to room temperature, transfer the product to a centrifuge, centrifuge at a speed of 6000-10000 rpm for 1-5 minutes, pour off the supernatant, retain the lower layer product, and then wash the lower layer product with high-purity water and ethanol for 3-5 times; then place the obtained solid product in a forced air drying oven, adjust the heating rate to 5°C / min, and dry it in a forced air drying oven at 50-80°C for 5-24 hours to obtain the target Mg3(OH)4(NO3)2 material; the corresponding card number of the X-ray diffraction is 26-1221, and the crystal plane index corresponding to the strongest peak is (100); the product belongs to the orthorhombic system, and the unit cell parameter is α=β=γ=90.0°; the microstructure is measured by field emission scanning electron microscope (SEM) at different magnifications and is found to be an ultra-thin nanosheet with a thickness of 60 to 100 nm and a diameter of 200 to 300 nm.