A self-compacting high-strength and high-toughness cement-based concrete repair material and preparation method thereof

By optimizing the raw material ratio and PVA fiber modification in cement-based repair materials, the problem of difficulty in balancing the strength and fluidity of cement-based repair materials is solved, achieving a combination of high strength, high toughness and high fluidity, which is suitable for construction Structural reinforcement design.

CN116143465BActive Publication Date: 2024-10-01XIAMEN ANNENG CONSTR +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211442091.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-17
Publication Date
2024-10-01
Estimated Expiration
2042-11-17

AI Technical Summary

Technical Problem

Existing cement-based concrete repair materials are difficult to maintain high fluidity when improving strength and toughness, and it is difficult to achieve high strength and high fluidity at the same time, which affects the construction convenience and performance of repair materials.

Method used

Using a specific ratio of Portland cement, mineral powder, fly ash, PVA fiber and other raw materials, and through the modification of PVA fiber, combined with the appropriate water-cement ratio and mortar-sand ratio, a self-compacting, high-strength and high-performance Tough cement-based repair material ensures that the material has high early strength, compressive strength, flexural strength and good fluidity with low PVA fiber addition.

Benefits of technology

It achieves high compressive strength, flexural strength and fluidity of cement-based repair materials. The 28d compressive strength exceeds 100MPa, the flexural strength reaches or exceeds 20.5MPa, the folding compression ratio exceeds 0.2, and the fluidity reaches or exceeds 250mm, which is significant. Improved the mechanical properties of the material and construction convenience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003948732210000091
    Figure BDA0003948732210000091
  • Figure BDA0003948732210000101
    Figure BDA0003948732210000101
  • Figure BDA0003948732210000102
    Figure BDA0003948732210000102
Patent Text Reader

Abstract

The present application relates to the field of cement materials, and specifically provides a self-compacting high-strength and high-toughness cement-based repair material and a preparation method thereof. The self-compacting high-strength and high-toughness cement-based repair material is composed of the following raw material components by weight: 300-350 parts of silicate cement, 90-110 parts of mineral powder, 70-80 parts of fly ash, 1-1.5 parts of water reducer, 0.3-0.5 parts of defoamer, 0.05-0.1 parts of cellulose, 27-32 parts of expansion agent, 10-15 parts of PVA fiber, 300-350 parts of sand and 100-115 parts of water. The self-compacting high-strength and high-toughness cement-based repair material of the present application has the characteristics of good fluidity, high compressive strength, flexural strength and flexural-compression ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cement materials, and more specifically, to a self-compacting high-strength and high-toughness cement-based concrete repair material and a preparation method thereof. Background Art

[0002] The strength of early concrete is low, resulting in a large number of early buildings now in urgent need of repair and reinforcement. For low-strength concrete components, the use of surface thin layer repair and reinforcement methods can minimize the impact on the appearance and use function of the original building. However, the following requirements are put forward for the concrete used for repair: good fluidity, early strength, high strength and toughness, good durability, strong impermeability, etc.

[0003] Adding PVA fiber to concrete can significantly improve the strength, toughness, and impermeability of concrete. However, the added PVA fiber will affect the fluidity of concrete. If the amount added is too much, the fluidity of concrete will be poor, and if the amount added is too little, the strength and toughness of concrete will not be significantly improved. Summary of the invention

[0004] The inventors found that directly adding PVA fibers to concrete in an amount exceeding 3% of the weight of the concrete would significantly affect the fluidity of the concrete, and the dispersion would be poor, and there would be obvious agglomeration, resulting in deterioration of the mechanical properties of the concrete. Based on this, the inventors analyzed the various raw materials of the concrete and conducted a large number of experiments, and found a high-strength and high-toughness cement-based repair material with high fluidity and a preparation method thereof. At a lower amount of PVA fiber added, the high fluidity of the concrete is maintained, and the concrete has high early strength, high compressive strength, high flexural strength, high fold-to-compression ratio and other properties.

[0005] Based on this, the present application provides a self-compacting high-strength and high-toughness cement-based repair material and a preparation method thereof.

[0006] This application adopts the following technical solutions:

[0007] A self-compacting high-strength and high-toughness cement-based repair material is composed of the following raw material components, measured by weight: 300-350 parts of silicate cement, 90-110 parts of mineral powder, 70-80 parts of fly ash, 1-1.5 parts of water reducer, 0.3-0.5 parts of defoamer, 0.05-0.1 parts of cellulose, 27-32 parts of expansion agent, 10-15 parts of PVA fiber, 300-350 parts of sand and 100-115 parts of water.

[0008] Preferably, the silicate cement is P·I62.5R grade silicate cement.

[0009] Preferably, the weight proportion of the PVA fiber in the raw material components is 1 to 1.5%.

[0010] Preferably, the cellulose is selected from ether cellulose, and the viscosity of a 1 wt % aqueous solution at 25° C. is 300 to 500 mPa.s.

[0011] Preferably, the water-to-cement ratio of the cement-based repair material is 0.2 to 0.22.

[0012] Preferably, the mortar-sand ratio of the cement-based repair material is 1.45 to 1.6.

[0013] Preferably, the PVA fiber is modified as follows:

[0014] The surface of the PVA fiber is subjected to corona treatment or plasma treatment to obtain treated PVA fiber;

[0015] The treated PVA fiber is treated with an aminosilane coupling agent to obtain an amino-modified PVA fiber;

[0016] The amino-modified PVA fibers are dispersed in an organic solvent and a solvent having a chemical formula of (CH 2 CH)OCH 2 O(PO) m (EO) n R single-ended epoxy polyether to react; wherein PO represents -CH 2 CH 3 CHO-, EO stands for -CH 2 CH 2 O-, m≥10, n≥5, R is C1-C4 alkyl or H.

[0017] More preferably, the ratio of the molar number of amino groups in the amino-modified PVA fiber to the molar number of the single-ended epoxy polyether is 1:0.5-3.

[0018] More preferably, the m is not higher than 100, the n is not higher than 70, and the difference between the m and the n is not higher than 30.

[0019] A method for preparing a self-compacting high-strength and high-toughness cement-based repair material according to any of the above embodiments comprises the following steps:

[0020] 1) dry-mixing the sand and the PVA fiber;

[0021] 2) adding the silicate cement, the mineral powder, the fly ash, the cellulose and the expansion agent, and dry-mixing and mixing to obtain a dry mix;

[0022] 3) The water reducing agent, the defoaming agent and the water are stirred and mixed, and then poured into the dry mix obtained in step 2), and mixed evenly to obtain the self-compacting high-strength and high-toughness cement-based concrete repair material.

[0023] In summary, this application has the following beneficial effects:

[0024] 1. The present application uses mineral powder and fly ash. The mineral powder has high activity and can improve the flexural strength and density of the repair material. Most of the fly ash is spherical and has a smooth surface. The inventors found that the addition of fly ash in the present application can improve the fluidity of the repair material due to its smooth spherical surface, and fly ash can improve the compressive strength of the repair material, which is beneficial to improving the fold-to-compression ratio and durability. When the weight ratio of fly ash to mineral powder is within a certain range, a cement-based repair material with good fluidity, flexural strength and compressive strength can be obtained.

[0025] 2. The application adds PVA fibers to concrete to play a role in tension. When the concrete matrix is ​​not cracked, the strong tension prevents the occurrence of cracks, and the concrete and PVA fibers are stressed synergistically; after cracks occur in the concrete matrix, the load is transferred to the PVA fibers, absorbing a large amount of energy, effectively improving the toughness of cement-based repair materials.

[0026] 3. The inventors found that further modification of PVA fibers with polyether can improve the bonding tightness between PVA fibers and concrete adhesive and enhance the mechanical properties of concrete; and the hydrophilic groups in polyether can increase the steric hindrance on the surface of cement particles, promote the dispersion of cement particles, release part of the encapsulated water, participate in the flow, and further improve the fluidity of the repair material.

[0027] 4. This application achieves a better combination of cement matrix and PVA fiber in the repair material through the selection of various raw materials and their weights, especially the selection of water-cement ratio and mortar-sand ratio, and solves the problem that high flexural strength, high compressive strength and high fluidity cannot coexist in cement-based repair materials. The cement-based repair material of this application can have a 28d compressive strength of more than 100MPa, a flexural strength of up to or exceeding 20.5MPa, a flexural-compression ratio of more than 0.2, and a fluidity of up to or exceeding 250mm, with excellent performance in various aspects. It achieves self-compacting, no vibration required, and convenient construction, providing a new type of cement-based repair material for the reinforcement design and construction of existing concrete structures that have extremely high requirements for strength, toughness and working performance. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below.

[0029] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0030] On the one hand, the present application provides a self-compacting high-strength and high-toughness cement-based repair material, which is composed of the following raw material components, by weight, 300-350 parts of silicate cement, 90-110 parts of mineral powder, 70-80 parts of fly ash, 1-1.5 parts of water reducer, 0.3-0.5 parts of defoamer, 0.05-0.1 parts of cellulose, 27-32 parts of expansion agent, 10-15 parts of PVA fiber, 300-350 parts of sand and 100-115 parts of water.

[0031] In the present application, the silicate cement is P·I62.5R grade silicate cement, which has high strength. The strength of P·I62.5R grade silicate cement is high, with a 3d compressive strength of 41.6MPa, a 28d compressive strength of 69.4MPa, a 3d flexural strength of 7.2MPa, and a 28d flexural strength of 8.8MPa. Using high-strength silicate cement as the base cement glue is conducive to obtaining a high-strength cement-based repair material.

[0032] Mineral powder is a highly active powder that can improve the pore structure of concrete and the interface structure of cement stone aggregate, improve the compressive strength of concrete, inhibit alkali-aggregate reaction, reduce hydration heat, reduce early temperature cracks in concrete structure, improve concrete density, and improve impermeability and erosion resistance. Further, the mineral powder is selected from ultrafine mineral powder with a particle size of no more than 1000 mesh, and further, the particle size is no more than 1500 mesh. Ultrafine mineral powder has higher activity and is more conducive to obtaining high-strength, self-compacting cement-based repair materials.

[0033] The large specific surface area and spherical micro-bead structure of fly ash have a significant promoting effect on improving the fluidity of cement-based repair materials and can also improve the flexural strength. Furthermore, the particle size of fly ash does not exceed 800 meshes.

[0034] Furthermore, the inventors found that the weight ratio of fly ash to mineral powder is 0.7 to 0.85:1, which makes the cement-based repair material of the present application have good fluidity, compressive strength and flexural strength. A weight ratio higher or lower than this range is not good for the compressive strength and flexural strength of the cement-based repair material. In particular, the flexural-compression ratio decreases significantly. Furthermore, the weight ratio of fly ash to mineral powder is 0.73 to 0.8:1.

[0035] The water reducing agent can improve the rheological properties of cement-based composite materials while maintaining the ratio of gel material to water, and improve the construction performance of cement-based composite materials while maintaining the mechanical properties. Furthermore, the water reducing agent can be selected from polycarboxylic acid-type water reducing agents.

[0036] The defoamer plays a role in breaking bubbles and reducing surface tension in the cement-based composite material of the present application. The use of the defoamer greatly improves the strength and stability of the hardened cement-based composite material, strengthens the matrix density, and improves the anti-permeability performance. Further, the defoamer can be a carboxylic acid defoamer.

[0037] In the present application, the functions of cellulose are water retention, thickening, thixotropy and air entrainment. Further, the cellulose is selected from ether cellulose, such as methyl cellulose ether, ethyl cellulose ether, etc. Further, the viscosity of 1wt% aqueous solution of cellulose at 25°C is 300-500mPa.s. The inventors found that in order to improve the fluidity of cement-based repair materials, the viscosity of cellulose cannot be large, otherwise it will significantly affect the fluidity.

[0038] The expansion agent can react to generate micro-expansion crystals, block capillary channels, and improve compactness and durability. In the present application, the expansion agent is a type I calcium sulphoaluminate concrete expansion agent.

[0039] In the present application, the sand is continuously graded, and the average particle size ranges from 0.3 to 0.6 mm. Continuously graded sand is a reasonable combination of sand particles of different sizes, which can not only obtain the minimum aggregate void ratio, but also the minimum aggregate specific surface area. The use of continuously graded sand can improve the strength and durability of concrete, and can also reduce the amount of cement used.

[0040] PVA fibers are commonly used as reinforcing components in high-strength concrete, which can effectively limit the development of initial cracks and improve the comprehensive performance of the matrix after hardening. In the present application, the weight proportion of PVA fibers in the raw material components is 1 to 1.5%. The inventors have found that adding more PVA fibers will significantly reduce the fluidity of the cement-based repair material of the present application.

[0041] The water-binder ratio refers to the ratio of the weight of water to the weight of silicate cement, mineral powder and fly ash. When the water-binder ratio is high, the fluidity of the cement-based repair material is good, but the mechanical strength will be reduced. When the water-binder ratio is low, the mechanical strength of the hydraulic-based repair material is high, but the fluidity will be poor. Too low a water-binder ratio is not conducive to the hydration of the cementitious material, which can easily cause defects inside the hardened matrix. The inventors found that the water-binder ratio of the cement-based repair material is 0.2-0.22, which can obtain a cement-based repair material with good comprehensive performance of fluidity and mechanical properties.

[0042] The mortar-sand ratio refers to the weight ratio of silicate cement, mineral powder and fly ash to the weight of sand. By controlling the mortar-sand ratio within an appropriate range, a cement-based repair material with good comprehensive performance in terms of fluidity and mechanical properties can be obtained. The inventors have found that the mortar-sand ratio of cement-based repair materials is more suitable at 1.45 to 1.6.

[0043] In this application, when the raw material components are determined, the main factors affecting the fluidity and mechanical strength of cement-based repair materials are PVA fiber content, water-cement ratio, mortar-sand ratio, weight ratio of fly ash to mineral powder, etc. The inventors conducted in-depth research and analysis on various influencing factors, and after a large number of experiments, obtained the technical solution of the self-compacting high-strength and high-toughness cement-based repair material of this application, which solved the problem that the fluidity and mechanical properties of cement-based repair materials cannot be achieved at the same time.

[0044] PVA fiber is an organic polymer material, and silicate, mineral powder, fly ash, etc. are inorganic non-metallic materials. PVA fiber has poor bonding with the above inorganic non-metallic materials. In order to further improve the effectiveness of PVA fiber, in this application, PVA fiber can be modified as follows:

[0045] The surface of the PVA fiber is subjected to corona treatment or plasma treatment to obtain treated PVA fiber;

[0046] The treated PVA fiber is treated with an aminosilane coupling agent to obtain an amino-modified PVA fiber;

[0047] The amino-modified PVA fibers are dispersed in an organic solvent and a solvent having a chemical formula of (CH 2 CH)OCH 2 O(PO) m (EO) n R single-ended epoxy polyether to react; wherein PO represents -CH 2 CH 3 CHO-, EO stands for -CH 2 CH 2 O-, m≥10, n≥5, R is C1-C4 alkyl or H.

[0048] In the above-mentioned PVA fiber modification method, the PVA fiber needs to be degreased before being treated with corona or plasma. The treatment can be carried out as follows: the PVA fiber is placed in an alkaline solution for ultrasonic degreasing, and then washed with clean water. The surface of the PVA fiber is inert. After being treated with corona or plasma, more active groups such as hydroxyl groups can be formed on the surface.

[0049] In the modification method of the PVA fiber, the aminosilane coupling agent can react with the hydroxyl group on the surface of the PVA fiber by utilizing its hydrolyzable alkoxy group, so that the surface of the PVA fiber carries an amino functional group, and the amino functional group can react with the epoxy group in the subsequent single-ended epoxy polyether, so that the polyether is grafted on the surface of the PVA fiber. There is no particular restriction on the aminosilane coupling agent that can be used. The aminosilane coupling agent contains at least one primary amino group in its molecular structure, and can be selected from 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, γ-aminoethylaminopropyltrimethoxysilane, γ-aminoethylaminopropyltriethoxysilane, etc. The specific operation of a modification method can be: adding 3-10 parts by weight of an aminosilane coupling agent to 90 parts by weight of an alcohol aqueous solution composed of anhydrous ethanol and water in a volume ratio of 9:1, stirring for 0.5-2 hours, then adding 1-5 parts by weight of the above-treated PVA fiber, continuing to stir for 1-2 hours, filtering, washing with deionized water, and drying to obtain amino-modified PVA fiber.

[0050] Further, the ratio of the molar number of amino groups in the amino-modified PVA fiber to the molar number of the single-ended epoxy polyether is 1:0.5-3. Further, the ratio of the molar number of amino groups in the amino-modified PVA fiber to the molar number of the single-ended epoxy polyether is 1:0.7-2.

[0051] In the present application, the reaction conditions of amino-modified PVA fiber and single-end epoxy polyether can be: adding 1% of 2-methylimidazole by weight of single-end epoxy polyether, and reacting at room temperature for 2 hours; or it can be that the reaction system of amino-modified PVA fiber and single-end epoxy polyether is heated to 50±℃ and reacted for 2 hours. After the reaction is completed, the filtered fiber is washed twice with anhydrous ethanol, left at room temperature for 2 hours, and then dried in an oven at 50℃ overnight.

[0052] In the above technical solution, m is not higher than 100, n is not higher than 70, and the difference between m and n is not higher than 30. If the values ​​of m and n are high, the molecular weight of the single-end epoxy polyether is large, and the activity of the epoxy group of the end group is low, which is not conducive to the reaction with the amino group on the surface of the PVA fiber, resulting in insufficient amount of polyether grafted on the surface of the PVA fiber. If the difference between m and n is large, the hydrophobic PO segment will affect the hydration of the hydrophilic EO segment, resulting in insufficient steric hindrance of the EO segment on the surface of the cement particles, and limited dispersion of the cement particles. Further, m is not higher than 50, and n is not higher than 25.

[0053] The inventors also found that in the above-mentioned single-ended epoxy polyether structure used in the present application, PO and EO are block structures, and the epoxy group is connected to the PO segment, that is, the PO segment is located in the middle of the epoxy group and the EO segment, and the effect of the polyether is better. It may be due to the reaction of the single-ended epoxy polyether with the amino group on the surface of the PVA fiber, the PO segment is closer to the PVA fiber than the EO segment, and the hydrophobic PO segment encapsulates the cement particles, which can make the PVA fiber and the cement particles closer and tighter. The hydrophilic EO segment extends more freely into the water, and the hydration range is larger, the steric hindrance is more obvious, and the stabilization effect is better. During the curing process of the cement-based repair material, as the water content decreases, the polyether segment is gradually wrapped on the surface of the cement particles. The polyether segment serves as a connecting structure between the PVA fiber and the cement particles, which improves the binding of the PVA fiber and the cement particles and the interaction between the PVA fiber and the cement particles, which not only improves the tensile strength (i.e., compressive strength) of the cement-based repair material, but also the polyether segment encapsulates the cement particles, which also improves the toughness (i.e., flexural strength) of the cement-based repair material.

[0054] Another aspect of the present application provides a method for preparing the self-compacting high-strength and high-toughness cement-based repair material described in any of the above embodiments, comprising the following steps:

[0055] 1) dry-mixing the sand and the PVA fiber;

[0056] 2) adding the silicate cement, the mineral powder, the fly ash, the cellulose and the expansion agent, and dry-mixing and mixing to obtain a dry mix;

[0057] 3) The water reducing agent, the defoaming agent and the water are stirred and mixed, and then poured into the dry mix obtained in step 2), and mixed evenly to obtain the self-compacting high-strength and high-toughness cement-based concrete repair material.

[0058] The following is a detailed description of the self-compacting high-strength and high-toughness cement repair material and its preparation method in combination with the embodiments, comparative examples and experimental data. The following raw material parts are parts by weight.

[0059] In the following embodiments, the silicate cement is P·I62.5R grade silicate cement, the average particle size of the continuously graded sand is 0.44 mm, the water reducer is Point-400S water reducer, the defoamer is a carboxylic acid defoamer, methyl cellulose ether (1wt% aqueous solution has a viscosity of 400mPa.s at 25°C), the expansive agent is type I calcium sulfoaluminate concrete expansive agent, the ultrafine mineral powder is 1500 mesh, the fly ash is 1000 mesh, and the PVA fiber is purchased from commercially available products.

[0060] Example 1

[0061] The self-compacting high-strength and high-toughness cement-based repair material is composed of 310 parts of silicate cement, 95 parts of mineral powder, 72 parts of fly ash, 1.2 parts of water reducer, 0.35 parts of defoamer, 0.07 parts of cellulose, 30 parts of expansion agent, 10 parts of PVA fiber, 300 parts of sand and 102 parts of water.

[0062] Example 2

[0063] The self-compacting high-strength and high-toughness cement-based repair material consists of 350 parts of silicate cement, 108 parts of mineral powder, 80 parts of fly ash, 1.3 parts of water reducer, 0.45 parts of defoamer, 0.1 parts of cellulose, 32 parts of expansion agent, 15 parts of PVA fiber, 350 parts of sand and 115 parts of water.

[0064] Example 3

[0065] The self-compacting high-strength and high-toughness cement-based repair material consists of 320 parts of silicate cement, 100 parts of mineral powder, 76 parts of fly ash, 1.2 parts of water reducer, 0.4 parts of defoamer, 0.08 parts of cellulose, 30 parts of expansion agent, 12 parts of PVA fiber, 320 parts of sand and 108 parts of water.

[0066] Example 4

[0067] In Example 3, the PVA fiber is adjusted from 12 parts to 13 parts, and the other raw material components and weight parts remain unchanged.

[0068] Example 5

[0069] In Example 3, the PVA fiber is adjusted from 12 parts to 14.5 parts, and the other raw material components and weight parts remain unchanged.

[0070] Example 6

[0071] In Example 3, the PVA fiber is adjusted from 12 parts to 10 parts, and the other raw material components and weight parts remain unchanged.

[0072] Example 7

[0073] In Example 3, the fly ash is adjusted from 76 parts to 78 parts, and the other raw material components and weight parts remain unchanged.

[0074] Example 8

[0075] In Example 3, the fly ash is adjusted from 76 parts to 80 parts, and the other raw material components and weight parts remain unchanged.

[0076] Example 9

[0077] In Example 3, the amount of sand was adjusted from 320 parts to 340 parts, and the other raw material components and weight portions remained unchanged.

[0078] Example 10

[0079] After degreasing, the PVA fiber was treated with plasma, and then surface treated with 3-aminopropyltrimethoxysilane, and then with the chemical formula (CH 2 CH)OCH 2 O(PO) 18.4 (EO) 7.7 CH 3 The epoxy-terminated block polyether was reacted in tetrahydrofuran (20 times the weight of the block polyether) at a molar ratio of amino group to epoxy group of 1:1 for 2 hours, filtered, washed twice with anhydrous ethanol, left at room temperature for 2 hours, and then dried in an oven at 50°C overnight to obtain polyether-modified PVA fiber.

[0080] In Example 3, the PVA fiber is replaced by the polyether-modified PVA fiber in equal parts by weight, and the other raw material components and weights remain unchanged.

[0081] Embodiment 11

[0082] After degreasing, the PVA fiber was treated with plasma, and then surface treated with 3-aminopropyltrimethoxysilane, and then with the chemical formula (CH 2 CH)OCH 2 O(PO) 40.9 (EO) 23.7 The epoxy-terminated block polyether of H was reacted in tetrahydrofuran (20 times the weight of the block polyether) at a molar ratio of amino group to epoxy group of 1:1.5 for 2 hours, filtered, washed twice with anhydrous ethanol, left at room temperature for 2 hours, and then dried in an oven at 50°C overnight to obtain polyether-modified PVA fiber.

[0083] In Example 3, the PVA fiber is replaced by the polyether-modified PVA fiber in equal parts by weight, and the other raw material components and weights remain unchanged.

[0084] Example 12

[0085] In Example 11, the polyether-modified PVA fiber was adjusted from 12 parts to 14.5 parts, and the other raw material components and weight parts remained unchanged.

[0086] Comparative Example 1

[0087] In Example 3, the PVA fiber is adjusted from 12 parts to 8 parts, and the other raw material components and weight parts remain unchanged.

[0088] Comparative Example 2

[0089] In Example 3, the PVA fiber is adjusted from 12 parts to 18 parts, and the other raw material components and weight parts remain unchanged.

[0090] Comparative Example 3

[0091] In Example 3, the PVA fiber is adjusted from 12 parts to 21 parts, and the other raw material components and weight parts remain unchanged.

[0092] Comparative Example 4

[0093] In Example 11, the polyether-modified PVA fiber was adjusted from 12 parts to 8 parts, and the other raw material components and weight parts remained unchanged.

[0094] Comparative Example 5

[0095] In Example 11, the polyether-modified PVA fiber was adjusted from 12 parts to 21 parts, and the other raw material components and weight parts remained unchanged.

[0096] Comparative Example 6

[0097] After the plasma treatment, the PVA fiber was surface treated with 3-aminopropyltrimethoxysilane and then reacted with the chemical formula (CH 2 CH)OCH 2 O(EO) 8.2 (PO) 19.3 CH 3 The epoxy-terminated block polyether was reacted in tetrahydrofuran (20 times the weight of the block polyether) at a molar ratio of amino group to epoxy group of 1:1.5 for 2 hours, filtered, washed twice with anhydrous ethanol, left at room temperature for 2 hours, and then dried in an oven at 50°C overnight to obtain polyether-modified PVA fiber.

[0098] In Example 3, the PVA fiber is replaced by an equal weight of polyether-modified PVA fiber, and the other raw material components and weight proportions remain unchanged.

[0099] Comparative Example 7

[0100] After the plasma treatment, the PVA fiber was surface treated with 3-aminopropyltrimethoxysilane and then reacted with the chemical formula (CH 2 CH)OCH 2 O(EO) 17.7 (PO) 32.8 CH 3 The epoxy-terminated block polyether was reacted in tetrahydrofuran (20 times the weight of the block polyether) at a molar ratio of amino group to epoxy group of 1:1.5 for 2 hours, filtered, washed twice with anhydrous ethanol, left at room temperature for 2 hours, and then dried in an oven at 50°C overnight to obtain polyether-modified PVA fiber.

[0101] In Example 3, the PVA fiber is replaced by an equal weight of polyether-modified PVA fiber, and the other raw material components and weight proportions remain unchanged.

[0102] Comparative Example 8

[0103] In Example 3, the mineral powder is adjusted from 100 parts to 76 parts, the fly ash is adjusted from 76 parts to 100 parts, and the other raw material components and weight portions remain unchanged.

[0104] Comparative Example 9

[0105] In Example 3, the mineral powder is adjusted from 100 parts to 110 parts, the fly ash is adjusted from 76 parts to 66 parts, and the other raw material components and weight parts remain unchanged.

[0106] The self-compacting high-strength and high-toughness cement-based repair materials of Examples 1-12 and Comparative Examples 1-9 are prepared as follows: sand and PVA fiber (or polyether-modified PVA fiber) are dry-mixed; Portland cement, mineral powder, fly ash, cellulose and expansion agent are added, dry-mixed to obtain a dry mix; the water reducer, defoamer and water are stirred and mixed, and then poured into the dry mix obtained above and mixed evenly.

[0107] Table 1 Proportions of cement-based repair materials for Examples 1-12 and Comparative Examples 1-9

[0108]

[0109]

[0110] Fluidity test: Tested in accordance with national standard GB / T 2419-2005.

[0111] Flexural strength test: The specimens are cured for 28 days and then tested in accordance with the national standard GB / T 17671-2021.

[0112] Compressive strength test: After the specimen is cured for 1 day, it is tested in accordance with the national standard GB / T 17671-2021.

[0113] Second compressive strength test: After the specimens are cured for 28 days, they are tested in accordance with the national standard GB / T 17671-2021.

[0114] The flexural strength to compressive strength ratio is the ratio of the flexural strength to the compressive strength.

[0115] The results are shown in Table 2 below.

[0116] Table 2

[0117]

[0118]

[0119] Analyze the data in Table 2 above. Comparing Examples 3-6 and Comparative Examples 1-3, when other raw material components and weights are the same, within a certain content range of PVA fiber, the fluidity decreases with the increase of PVA fiber content, and the compressive strength and flexural strength increase with the increase of PVA fiber content. However, when the content of PVA fiber is low (0.83% in Comparative Example 1) or high (1.85% in Comparative Example 2, 2.15% in Comparative Example 3), the fluidity, compressive strength and flexural strength change greatly, especially when the content is high, the compressive strength and flexural strength become lower, and the flexural-compression ratio is also lower than 0.2. This may be due to the poor dispersibility of PVA fiber in cement-based repair materials. When the amount added is large, it is difficult to disperse well, and there is obvious agglomeration. PVA agglomeration has an adverse effect on the mechanical properties of cement-based repair materials.

[0120] Comparing Examples 10 and 11 with Comparative Examples 1 and 3-5, when the content of PVA fibers exceeds a certain range, even if the PVA fibers are modified with polyether, there is no substantial improvement in the performance of cement-based repair materials. Especially when the content of PVA fibers is high, the use of polyether-modified PVA cannot solve the dispersion problem caused by agglomeration.

[0121] Comparing Examples 3, 7, 8 with Comparative Examples 8, 9, with the same other raw material components and weights, as the weight ratio of fly ash to mineral powder is adjusted, when the weight ratio of fly ash to mineral powder exceeds a certain range, the compressive strength, flexural strength and flexural-compression ratio all deteriorate.

[0122] Comparative Examples 3, 10, 11 and Comparative Examples 6 and 7, with the same other raw material components and weights, after the PVA fiber is surface treated with polyether, the fluidity and mechanical properties of the cement-based repair material are improved. This is because the polyether can improve the compatibility of the PVA fiber with cement, and the polyether with a specific structure also helps to further improve the dispersibility of the cement particles, indicating that the polyether in which the epoxy group is adjacent to the PO segment in the polyether structure can play a better role, and the fluidity and mechanical properties are better.

[0123] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A self-compacting high-strength and high-toughness cement-based repair material, Features: The raw material composition is composed of the following raw material components by weight: 300-350 parts of silicate cement, 90-110 parts of mineral powder, 70-80 parts of fly ash, 1-1.5 parts of water reducing agent, 0.3-0.5 parts of defoaming agent, 0.05-0.1 parts of cellulose, 27-32 parts of expansion agent, 10-15 parts of PVA fiber, 300-350 parts of sand and 100-115 parts of water; The weight proportion of the PVA fiber in the raw material components is 1 to 1.5%; The water-cement ratio of the cement-based repair material is 0.2 to 0.22; The mortar-sand ratio of the cement-based repair material is 1.45 to 1.6; The PVA fiber is modified as follows: The surface of the PVA fiber is subjected to corona treatment or plasma treatment to obtain treated PVA fiber; The treated PVA fiber is treated with an aminosilane coupling agent to obtain an amino-modified PVA fiber; The amino-modified PVA fibers are dispersed in an organic solvent and a solvent having a chemical formula of (CH 2 CH)OCH 2 O(PO) m (EO) n R single-ended epoxy polyether to react; wherein PO represents -CH 2 CH 3 CHO-, EO stands for -CH 2 CH 2 O-, m≥10, n≥5, R is a C1-C4 alkyl group or H; the ratio of the molar number of amino groups in the amino-modified PVA fiber to the molar number of the single-ended epoxy polyether is 1:0.5-3; the m is not higher than 100, the n is not higher than 70, and the difference between the m and the n is not higher than 30.

2. The self-compacting high-strength and high-toughness cement-based repair material according to claim 1, Features: The silicate cement is P·Ⅰ62.5R grade silicate cement.

3. The self-compacting high-strength and high-toughness cement-based repair material according to claim 1, Features: The cellulose is selected from ether cellulose, and the viscosity of a 1 wt % aqueous solution at 25° C. is 300 to 500 mPa.s.

4. A method for preparing the self-compacting high-strength and high-toughness cement-based repair material according to any one of claims 1 to 3, Features: The following steps are included: 1) dry-mixing the sand and the PVA fiber; 2) adding the silicate cement, the mineral powder, the fly ash, the cellulose and the expansion agent, and dry-mixing and mixing to obtain a dry mix; 3) The water reducing agent, the defoaming agent and the water are stirred and mixed, and then poured into the dry mix obtained in step 2), and mixed evenly to obtain the self-compacting high-strength and high-toughness cement-based concrete repair material.