Imidazole functionalized composite anion exchange membrane and its preparation method and application
By treating the surface of the porous base film and introducing 1,2,4,5-tetramethylimidazole functional groups on the solvent-free in-situ thermal polymerization method, the problem of poor chemical stability of anion exchange membrane in an alkaline environment is solved, and the problem of poor chemical stability of anion exchange membrane in an alkaline environment is improved. The mechanical properties and chemical stability of the membrane are reduced, the risk of pollution is achieved, and the airtightness and electrical conductivity are achieved.
Patent Information
- Application Number
- CN202211610687.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-12
AI Technical Summary
The existing anion exchange membrane has poor chemical stability in alkaline environments, resulting in a short service life and a risk of contamination and human damage during the preparation process.
In situ polymerization and crosslinking of monomers are achieved in porous base membrane pores by solvent-free in situ thermal polymerization, and the introduction of highly chemically stable 1,2,4,5-tetramethylimidazole functional groups are porous at different thicknesses. Prepare imidazole functionalized composite anion exchange membrane by surface treatment of base film to enhance the chemical stability and mechanical strength of the membrane.
It improves the chemical stability and mechanical properties of the anion exchange membrane, reduces the risk of contamination and human damage during preparation and use, and achieves higher airtightness and electrical conductivity.
Smart Images

Figure BDA0003994999680000021 
Figure FDA0003994999670000011 
Figure HDA0003994999690000011
Abstract
Description
Technical Field
[0001] The invention relates to an imidazole functionalized composite anion exchange membrane and a preparation method and application thereof, belonging to the field of fuel cells and electrolytic cells. Background Art
[0002] With the global consumption of fossil energy, the demand for renewable energy is increasing day by day. The development of efficient, clean and sustainable new energy conversion technologies has become a trend. Fuel cells, as a new energy technology, directly convert the chemical energy of fuels (such as hydrogen or methanol) into zero-emission, high-energy conversion electrical energy. Vehicles and mobile devices using proton exchange membrane fuel cells (PEMFC) have been commercialized. However, due to the high cost of PEMFC and its heavy reliance on platinum (Pt) catalysts, its widespread application is hindered. Compared with PEMFC, anion exchange membrane fuel cells (AEMFC) operating under alkaline conditions have the cost advantages of using non-platinum group metal (non-PGM) catalysts and cheap bipolar plates. At present, AEMFC has made significant progress, especially in terms of power density, reaching a level comparable to PEMFC, but it is currently difficult for AEMFC to achieve long-term stable operation. The low chemical stability of the anion exchange membrane (AEM), which is the core component of AEMFC, is one of the main factors that prevent AEMFC from operating for a long time. The main reason for the poor chemical stability of AEM is that its organic cationic groups undergo severe degradation in an alkaline environment. Therefore, improving the stability of organic cations is the main way to improve the chemical stability of AEM, which is of great significance to improving the operating stability of AEMFC.
[0003] Composite membrane enhancement technology is an effective way to improve the mechanical strength of the membrane, so that the film still has good mechanical properties.
[0004] At present, there are a lot of research on composite anion exchange membranes. The Chinese invention patent "Ultra-thin cross-linked composite reinforced polymer anion exchange membrane and its preparation method and application" (patent application number: 201811436085.2) discloses a composite membrane functionalized with trimethylamine; the Chinese invention patent application "A method for preparing an ultra-thin composite anion exchange membrane" (patent application number: 202110442464.8) discloses a composite membrane functionalized with N-methylpiperidine. Both of the above methods have defects: (1) The above functional groups are used for functionalization. The quaternary ammonium group has a strong odor and is harmful to the human body. There is a risk of polluting the environment and damaging the human body during the preparation and use of the membrane; (2) The above functional groups have low chemical stability in an alkaline environment, resulting in a short service life of the membrane. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide an imidazole functionalized composite anion exchange membrane and its preparation method and application in view of the shortcomings of the current anion exchange membrane, such as poor chemical stability and insufficient mechanical properties. The present invention realizes in-situ polymerization and cross-linking of monomers in the pores of the porous base membrane by a solvent-free in-situ thermal polymerization method based on the surface treatment of porous base membranes of different thicknesses. Porous base membranes of different thicknesses can be used to prepare composite membranes with different mechanical strengths to meet the requirements of electrochemical energy devices for the mechanical strength of anion exchange membranes; in-situ thermal polymerization can make the composite membrane more compact and ensure the air tightness of the composite membrane. The chemical stability of the anion exchange membrane is improved by introducing highly chemically stable 1,2,4,5-tetramethylimidazole functional groups into the reinforced composite membrane, thereby reducing the risk of pollution and damage to the human body during preparation and use.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] The present invention provides an imidazole functionalized composite anion exchange membrane, the molecular structure of which is as follows:
[0008]
[0009] In the formula, x=94~98, y=2~6, z=2~8.
[0010] The present invention also provides a method for preparing an imidazole functionalized composite anion exchange membrane, comprising the following steps:
[0011] (1) Pretreatment of porous basement membrane: the porous basement membrane is treated with ethanol and dried;
[0012] (2) Preparation of polymer monomer mixture
[0013] The dibenzoyl peroxide is subjected to a water removal treatment, and chloromethylstyrene, divinylbenzene and hexafluorobutyl methacrylate are respectively passed through a basic alumina solid extraction column to remove the polymerization inhibitor; the molar ratio of chloromethylstyrene: divinylbenzene: hexafluorobutyl methacrylate is 94-98: 2-6: 2-8, and then stirred, and the mass ratio is chloromethylstyrene: dibenzoyl peroxide is 1: 0.01-0.03, and dibenzoyl peroxide is added, and the mixture is stirred for reaction to obtain a polymer monomer mixed solution;
[0014] (3) Preparation of enhanced composite membrane
[0015] Under normal temperature conditions, the porous base film obtained in step (1) is laid flat on a peelable polyester sheet, and the polymer monomer mixture obtained in step (2) is added to the porous base film. After the polymer monomer mixture completely soaks the porous base film, another peelable polyester sheet is covered on the porous base film to drive out bubbles; hot pressing, cooling and removing the peelable polyester sheet to obtain a reinforced composite membrane;
[0016] (4) Preparation of imidazole functionalized composite anion exchange membrane
[0017] The enhanced composite membrane prepared in step (3) is immersed in a 20-50 wt% imidazole compound solution at 40-60° C. for 3-6 days, washed and dried to obtain a chloride ion type composite anion exchange membrane; the chloride ion type composite anion exchange membrane is immersed in a 0.5-2 mol L -1 The membrane is immersed in a KOH solution for 12 to 36 hours and then washed to obtain a hydroxide-type imidazole functionalized composite anion exchange membrane.
[0018] Furthermore, the porous base membrane pretreatment includes: immersing the porous base membrane in an ethanol solution, maintaining it at room temperature for 1 to 5 hours, and then washing it with ethanol 2 to 5 times, so as to remove dust and other impurities on the porous base membrane and perform hydrophilic treatment on it, and then drying it under vacuum conditions and storing it in a dust-free sealed bag for future use.
[0019] Furthermore, the porous base membrane includes a polyethylene membrane with a porosity of 36-46%, a polypropylene membrane with a porosity of 50-60%, or a polytetrafluoroethylene membrane with a porosity of 80-90%.
[0020] Furthermore, the thickness of the polyethylene film is 5.5 to 20 μm, the thickness of the polypropylene film is 22 to 25 μm, and the thickness of the polytetrafluoroethylene film is 8 to 20 μm.
[0021] Furthermore, in step (2), the stirring conditions after mixing chloromethylstyrene, divinylbenzene and hexafluorobutyl methacrylate are 10 to 20 minutes at room temperature; and the stirring conditions after adding dibenzoyl peroxide are 1 to 2 hours at room temperature.
[0022] Furthermore, the conditions of the hot pressing in step (3) are: pressure 1-3 MPa, temperature 80-100° C., and time 8-16 h.
[0023] Furthermore, the imidazole compound includes 1,2,4,5-tetramethylimidazole, and the solvent for preparing the imidazole compound solution includes tetrahydrofuran, ethanol, etc.;
[0024] The cleaning comprises: washing with deionized water for 2 to 5 times, then soaking in deionized water for 6 to 12 hours, and then washing with deionized water for 2 to 5 times;
[0025] The drying temperature is 40-60°C.
[0026] The present invention also provides an application of the imidazole functionalized composite anion exchange membrane or the imidazole functionalized composite anion exchange membrane prepared by the above preparation method, which is applied to anion exchange membrane fuel cells.
[0027] The invention avoids the existence of quaternary ammonium groups that pollute the environment and harm the human body during the preparation and use process, has relatively safe operation and simple process.
[0028] The present invention uses 1,2,4,5-tetramethylimidazole for functionalization to improve the chemical stability of the anion exchange membrane.
[0029] The present invention adopts a preparation method with a low cross-linking degree (DVB: 2-6), and the composite membrane fully swells during the functionalization process, avoiding the problem that 1,2,4,5-tetramethylimidazole is too large and difficult to enter the membrane for reaction, so that the composite membrane can be fully functionalized; at the same time, the low cross-linking degree improves the conductivity of the membrane without losing air tightness. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 FTIR spectra of the PE porous base membrane (a), the enhanced composite membrane prepared in Example 2 (b), and the PE composite anion exchange membrane (c).
[0031] Figure 2 SEM images of the PE porous base membrane and the PE composite anion exchange membrane prepared in Example 2; Figures a and b are the plan and cross-sectional SEM images of the PE porous base membrane, and c and d are the plan and cross-sectional SEM images of the PE composite anion exchange membrane prepared in Example 2.
[0032] Figure 3 It is a mechanical property diagram of the PE porous base membrane and the PE composite anion exchange membrane prepared in Example 2; Curve 1 represents the PE porous base membrane, and Curve 2 represents the ultra-thin composite anion exchange membrane prepared in Example 2.
[0033] Figure 4 H is the H of the PE composite anion exchange membrane prepared in Example 2 2 / O 2 Power density curve of alkaline fuel cell.
[0034] Figure 5 This is the hydrogen permeation current curve of the PE composite anion exchange membrane prepared in Example 2. DETAILED DESCRIPTION
[0035] The preparation method of the PE composite anion exchange membrane of the present invention is further described in detail below through specific embodiments.
[0036] Example 1
[0037] A method for preparing an imidazole functionalized composite anion exchange membrane, comprising the following steps:
[0038] (1) Pretreatment of porous base membrane
[0039] The wet PE (8 μm) porous base membrane was cut into appropriate shapes, immersed in an ethanol solution, kept at room temperature for 3 hours, and then washed with ethanol 3 times to remove dust and other impurities on the porous base membrane and perform hydrophilic treatment on it. It was then dried under vacuum conditions and stored in a dust-free sealed bag for later use.
[0040] (2) Preparation of polymer monomer mixture
[0041] High-purity (purity greater than 99%) dibenzoyl peroxide (BPO) is stored in a silica gel desiccant for dehydration treatment; chloromethylstyrene (VBC), divinylbenzene (DVB) and hexafluorobutyl methacrylate (HFM) are respectively extracted through an alkaline alumina (ALB) solid extraction column to remove the polymerization inhibitor, thereby obtaining purified VBC, DVB and HFM, which are then stored in a low-temperature environment for future use; the purified VBC, DVB and HFM are respectively weighed in a molar ratio of VBC:DVB:HFM=0.98:0.02:0.02, added into a sealable single-necked flask, stirred at room temperature for 15 to 20 minutes, and then BPO weighed in a mass ratio of VBC:BPO=1:0.01 is added thereto, and stirring is continued for 1.5 to 2 hours at room temperature to obtain a polymer monomer mixture.
[0042] (3) Preparation of enhanced composite membrane
[0043] The PE porous base film treated in step (1) is laid flat on a peelable polyester sheet. Under room temperature, the polymer monomer mixture prepared in step (2) is dripped onto the PE porous base film. After the mixture completely soaks the PE porous base film, another peelable polyester sheet is covered on the PE porous base film to form a "sandwich" structure. The bubbles therein are then driven out by a scraping rod. This squeezing force can also make the polymer monomer mixture and the PE porous base film further adhere. After standing for 30 to 40 minutes, the excess mixture on the surface of the PE porous base film is again driven out by a scraping rod. This operation is repeated to prepare multiple composite films. The composite film with the "sandwich" structure is placed on an oil press at a pressure of 1 MPa, heated to 90°C and maintained for 14 to 16 hours, cooled to room temperature, and the polyester sheets on both sides are removed to obtain a reinforced composite film.
[0044] (4) Preparation of 1,2,4,5-tetramethylimidazole (TMI) functionalized PE composite anion exchange membrane
[0045] The reinforced composite membrane prepared in step (3) is immersed in a 60°C, 30 wt% 1,2,4,5-tetramethylimidazole tetrahydrofuran solution for 6 days, then washed with deionized water for 2 to 3 times, then immersed in deionized water for 6 to 12 hours, then washed with deionized water for 2 to 3 times, and dried in a vacuum drying oven at 40 to 60°C for 24 hours to obtain a chloride ion type composite anion exchange membrane; the chloride ion type composite anion exchange membrane is immersed in a 1 mol L -1 The membrane was immersed in a KOH solution for 24 hours, washed with deionized water for 2 to 3 times, and stored in deionized water for later use to obtain a hydroxide-type 1,2,4,5-tetramethylimidazole functionalized composite anion exchange membrane.
[0046] Example 2
[0047] (1) Use a wet PE (12 μm) porous base membrane to carry out (1), (2), (3), and (4) in Example 1.
[0048] Figure 1 FTIR spectra of PE porous base membrane (a), enhanced composite membrane prepared in Example 2 (b) and PE composite anion exchange membrane (c), the horizontal axis is wave number (cm -1 ), the vertical axis is the transmittance. Curve a: 2914.89cm -1 Asymmetric stretching vibration of methylene CH, 2848.18 cm -1 Symmetric stretching vibration of methylene CH, 1452.88 and 1472.14 cm -1 The bending vibration of methylene CH, 717.60 and 730.60 cm -1 The rocking vibration of methylene CH indicates polyethylene. Curve b: 1366.96, 1183.64 and 824.86 cm -1 For CF 2 , CF and CF 3 The characteristic peak is 1722.11cm -1 It is the characteristic absorption peak of C=O, 1095.97cm -1 It is the characteristic absorption peak of COC; 1264.58cm -1 CH 2 The characteristic absorption peak of Cl is 675.24 cm -1 It is the characteristic peak of benzene ring, and the surface hexafluorobutyl methacrylate and chloromethylstyrene are successfully compounded. Curve c: 3361.85cm -1 is the stretching vibration of CH on the imidazole ring, 1650.99 is the stretching vibration of C=N and C=C, 1537.23cm -1 N=CN stretching vibration, 808.07cm-1 The peaks are the vibration peaks of nitrogen heterocyclic ring, indicating that 1,2,4,5-tetramethylimidazole was successfully functionalized.
[0049] (2) Morphological representation
[0050] The PE composite anion exchange membrane sample and the PE porous base membrane sample prepared in step (1) were cut into appropriate sizes, fractured in liquid nitrogen, vacuum-sprayed with gold for 30 seconds, and then observed under a scanning electron microscope (FE-SEM: JSM-6700F) at a voltage of 10 kV. The results are as follows: Figure 2 shown.
[0051] Thermal polymerization without solvent evaporation makes the porous PE membrane fully filled with electrolyte, as shown in the cross-sectional view, but small surface molecules fall off during the functionalization process to form small pits, as shown in the plan view.
[0052] (3) Mechanical properties test
[0053] The PE composite anion exchange membrane and PE porous base membrane prepared in step (1) were dried in a vacuum drying oven at 60°C for 24 hours, and then cut into samples of 1 cm×5 cm. The test was carried out using a universal testing machine (WDW-100) at room temperature and a tensile rate of 10 mm / min, and the following results were obtained: Figure 3 The maximum tensile strength of the composite film is 152.86 MPa (not lower than 151.25 MPa of PE porous film), and the elongation at break is 152.71% (lower than 177.87% of PE).
[0054] (4) Fuel cell performance test
[0055] First, weigh appropriate amounts of 70 wt% Pt / C and 60 wt% PtRu / C catalysts respectively and add them to a sample bottle, then add an ionomer (5 wt% DMSO solution), and then add a 40-60 times the mass of the catalyst n-propanol solution, and ultrasonicate the sample bottle in a water bath for 2-3 h to form a catalyst ink; take out a 3 cm×4 cm composite anion exchange membrane prepared in step (1), and spray the prepared Pt / C and PtRu / C catalyst inks on both sides of the membrane to form a cathode catalyst layer and an anode catalyst layer, and the catalyst loading is 0.4 mg / cm 2 , which is the CCM (catalyst-coated membrane) membrane electrode; finally, the prepared CCM was installed in a 2×2.5 cm 2The fuel cell test system was used to test the battery performance in a single cell. The test conditions were: battery temperature 60°C, pure hydrogen as fuel, pure oxygen as oxidant, back pressure of both cathode and anode was 0.1MPa, and gas flow of both anode and cathode was 0.5L / min. The single cell power test was performed, and the test results are as follows: Figure 4 As shown. The single cell current density is 586.4 mA cm -2 The maximum power density is 358.70 mW cm -2 , and has good performance. And the open circuit voltage is above 1.0V, indicating that the membrane has good fuel barrier ability.
[0056] (5) Hydrogen permeation current test
[0057] After testing the single cell performance of the battery, the cathode gas flow was changed to nitrogen, and the battery was purged under other conditions. When the open circuit voltage dropped to about 0.1V and stopped decreasing, Gamry selected the Linear Sweep Voltammetry (LSV) mode to measure the hydrogen permeation of the battery. The parameters during the test were: scan range 0-0.6V, scan rate 10mV / s. The test results are as follows: Figure 5 When the voltage is 400mV, the hydrogen permeation current is 1.40mA / cm 2 , less than 2.0mA / cm 2 , indicating that the membrane has good fuel barrier ability.
Claims
1. An imidazole functionalized composite anion exchange membrane, characterized in that: The molecular structure is as follows: In the formula, x=94~98, y=2~6, z=2~8.
2. A method for preparing an imidazole functionalized composite anion exchange membrane, characterized in that: The steps include: (1) Pretreatment of porous basement membrane: the porous basement membrane is treated with ethanol and dried; (2) Preparation of polymer monomer mixture The dibenzoyl peroxide is subjected to a water removal treatment, and chloromethylstyrene, divinylbenzene and hexafluorobutyl methacrylate are respectively passed through a basic alumina solid extraction column to remove the polymerization inhibitor; the molar ratio of chloromethylstyrene: divinylbenzene: hexafluorobutyl methacrylate is 94-98: 2-6: 2-8, and then stirred, and the mass ratio is chloromethylstyrene: dibenzoyl peroxide is 1: 0.01-0.03, and dibenzoyl peroxide is added, and the mixture is stirred for reaction to obtain a polymer monomer mixed solution; (3) Preparation of enhanced composite membrane Under normal temperature conditions, the porous base film obtained in step (1) is laid flat on a peelable polyester sheet, and the polymer monomer mixture obtained in step (2) is added to the porous base film. After the polymer monomer mixture completely soaks the porous base film, another peelable polyester sheet is covered on the porous base film to drive out bubbles; hot pressing, cooling and removing the peelable polyester sheet to obtain a reinforced composite membrane; (4) Preparation of imidazole functionalized composite anion exchange membrane The enhanced composite membrane prepared in step (3) is immersed in a 20-50 wt% imidazole compound solution at 40-60° C. for 3-6 days, washed and dried to obtain a chloride ion type composite anion exchange membrane; the chloride ion type composite anion exchange membrane is immersed in a 0.5-2 mol L -1 The membrane is immersed in a KOH solution for 12 to 36 hours and then washed to obtain a hydroxide-type imidazole functionalized composite anion exchange membrane.
3. The preparation method according to claim 2, characterized in that: The porous base film pretreatment comprises: immersing the porous base film in an ethanol solution, keeping it at room temperature for 1 to 5 hours, then washing it with ethanol for 2 to 5 times, and then drying it under vacuum conditions.
4. The preparation method according to claim 2, characterized in that: The porous base film includes a polyethylene film with a porosity of 36-46%, a polypropylene film with a porosity of 50-60%, or a polytetrafluoroethylene film with a porosity of 80-90%.
5. The preparation method according to claim 4, characterized in that: The thickness of the polyethylene film is 5.5 to 20 μm, the thickness of the polypropylene film is 22 to 25 μm, and the thickness of the polytetrafluoroethylene film is 8 to 20 μm.
6. The preparation method according to claim 2, characterized in that: In step (2), the stirring condition after mixing chloromethylstyrene, divinylbenzene and hexafluorobutyl methacrylate is 10 to 20 minutes at room temperature; and the stirring condition after adding dibenzoyl peroxide is 1 to 2 hours at room temperature.
7. The preparation method according to claim 2, characterized in that: The hot pressing conditions in step (3) are: pressure 1-3 MPa, temperature 80-100° C., and time 8-16 h.
8. The preparation method according to claim 2, characterized in that: The imidazole compound includes 1,2,4,5-tetramethylimidazole, and the solvent for preparing the imidazole compound solution includes tetrahydrofuran and ethanol; The cleaning comprises: washing with deionized water for 2 to 5 times, then soaking in deionized water for 6 to 12 hours, and then washing with deionized water for 2 to 5 times; The drying temperature is 40-60°C.
9. Use of the imidazole functionalized composite anion exchange membrane according to claim 1 or the imidazole functionalized composite anion exchange membrane prepared by the preparation method according to any one of claims 2 to 8, characterized in that: Applied to anion exchange membrane fuel cells.