A novel acetonitrile catalyst and preparation method thereof

The novel acetonitrile catalyst, using ZrO2 and WO3 on nano-scale porous carbon, addresses the limitations of existing catalysts by achieving high yield and extended service life, suitable for industrial applications.

CN116173942BActive Publication Date: 2024-12-06NANTONG LIYANG CHEM CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211719321.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-12-06
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Existing acetonitrile production catalysts suffer from poor catalyst activity, selectivity, and stability, limiting their conversion rate and yield, which impedes industrial application.

Method used

A novel acetonitrile catalyst composed of ZrO2 and WO3 supported on nano-scale porous carbon, utilizing waste straw as a raw material, enhances catalyst activity and selectivity, allowing for high yield and extended service life.

Benefits of technology

The catalyst achieves a yield of over 99% acetonitrile with a conversion rate of 99.99%, and can be reused multiple times, aligning with green chemical industry principles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004029270330000071
    Figure BDA0004029270330000071
Patent Text Reader

Abstract

The present invention relates to the field of chemical technology, in particular to IPC C07C255, and more specifically to a novel acetonitrile catalyst and a preparation method thereof. The present invention prepares zirconium nitrate and sodium tungstate aqueous solutions by adding zirconium nitrate and sodium tungstate to deionized water, respectively, and then adds nano-scale porous carbon, stirs, stands, dries, and calcines in two stages to obtain a zirconium-tungsten bimetallic porous carbon catalyst. The catalyst prepared by the present invention can maintain high activity and selectivity for a long time, and can be revived for multiple uses, so that the service life is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical industry, in particular to IPC C07C255, and more specifically to a novel acetonitrile catalyst and a preparation method thereof. Background Art

[0002] Acetonitrile, also known as methyl nitrile, is the single most saturated aliphatic nitrile. Due to its unique functional group nitrile, it has excellent solvent properties, can dissolve a variety of organic, inorganic and gaseous substances, and has a better distribution ratio and desorption ability. It has a certain toxicity and is infinitely miscible with water and alcohol. The carbon-nitrogen triple bond of acetonitrile is prone to typical nitrile reactions. Therefore, acetonitrile can not only be used as a solvent, but also can be used to produce many nitrogen-containing compounds. It is an important organic intermediate. The commonly used acetonitrile production methods are roughly divided into two categories: direct synthesis and indirect methods. The direct synthesis method includes more than ten synthesis methods such as carbon monoxide ammonia hydrogenation method and ethanol ammonia method. The indirect method is mainly the propylene ammoxidation by-product method.

[0003] There is an early international patent research: using phosphorus molybdenum heteropoly acid H 3 PMo 12 O 4 As a catalyst, the carrier can be silica, diatomaceous earth, silica gel, pumice or alumina, etc. Among the several carriers, silica gel has the best effect. 3 , the specific surface area is about 500m 2 / g silica gel is used as a carrier and coated with 10-35% 12-molybdophosphoric acid under suitable process conditions (reaction temperature is 380-420°C, the molar ratio of ethanol to ammonia is 1:(3-4), the residence time is 5s, and the evaluation is carried out under normal pressure. The ethanol conversion rate and acetonitrile selectivity are 96% and 65% respectively, which are low in conversion rate and selectivity and do not meet the process index standards.

[0004] Roger et al. of Cyanamid Company in the United States first reported the use of 15% Cu / Al 2 O 3 and 5%Cu5%Zn / Al 2 O 3 It can catalyze the synthesis of acetonitrile from ethanol. Under the optimal reaction conditions, the yield of acetonitrile can reach 87%, but still less than 99%.

[0005] The above documents and patents all have the problem of poor catalyst activity, selectivity and stability, which affects the conversion rate of raw materials and the yield of acetonitrile, and limits their prospects for industrial application. Summary of the invention

[0006] In order to solve the problems in the prior art, the present invention provides a novel acetonitrile catalyst in the first aspect, the composition of which includes ZrO2 , WO 3 , nanoscale porous carbon.

[0007] In some preferred embodiments, the ZrO 2 The mass percentage of the nano-porous carbon is 25-45%; further preferably, ZrO 2 The mass percentage of the nano-scale porous carbon is 30-40%.

[0008] In some preferred embodiments, the WO 3 Accounting for ZrO 2 and nano-porous carbon by mass percentage is 30-50%; further preferably, WO 3 Accounting for ZrO 2 The mass percentage of the nano-scale porous carbon is 35 to 45%.

[0009] The inventors found that by selecting nano-scale porous carbon as a catalyst carrier, the catalyst can be revived and used more often and its service life can be extended while maintaining the high activity and selectivity of the catalyst. The inventors creatively found that by selecting nano-scale porous carbon as a catalyst carrier, compared with single activated carbon or carbon fiber, it has a higher porosity and specific surface area, and the porous carbon modified by metal compounds has higher activity, catalytic performance and higher thermal stability. In addition, the nano-scale porous carbon uses waste straw as raw material and is carbonized by high-temperature calcination. Its source is green and environmentally friendly. At the same time, it can be calcined again after use to restore its activity and extend its service life.

[0010] The second aspect of the present invention provides a method for preparing a novel acetonitrile catalyst, comprising the following steps: adding zirconium nitrate and sodium tungstate (purchased from Sinopharm Chemical Reagent Co., Ltd., analytical grade) to deionized water to prepare zirconium nitrate and sodium tungstate aqueous solutions, respectively; adding nano-scale porous carbon to the zirconium nitrate aqueous solution, stirring, standing, drying, and calcining; and then placing it in a sodium tungstate aqueous solution, stirring, standing, drying, and calcining to obtain a zirconium-tungsten bimetallic porous carbon catalyst.

[0011] In some preferred embodiments, the specific method of preparing the novel acetonitrile catalyst comprises the following steps:

[0012] S1: adding zirconium nitrate to deionized water to prepare a zirconium nitrate aqueous solution;

[0013] S2: adding nano-porous carbon to the zirconium nitrate aqueous solution, stirring and mixing evenly to obtain a zirconium nitrate-porous carbon aqueous solution;

[0014] S3: Stir and evaporate the zirconium nitrate-porous carbon aqueous solution in a water bath at 70-100°C, dry it at 100-140°C overnight, take it out after drying, and calcine it to obtain 25-45% ZrO2 / APC;

[0015] S4: Add sodium tungstate into deionized water to prepare a sodium tungstate aqueous solution;

[0016] S5: Add 25-45% ZrO to the sodium tungstate aqueous solution. 2 / APC, stir and mix evenly, then stir and evaporate to dryness in a water bath at 85°C, dry overnight at 100-140°C, take out after drying, calcine, and obtain 25-45ZrO 2 / 35~45WO 3 / APC.

[0017] In some preferred embodiments, the zirconium nitrate in S1 is zirconium nitrate pentahydrate.

[0018] In some preferred embodiments, the stirring time of S2 is 1.5 to 3 hours;

[0019] In some preferred embodiments, the calcination temperature in S3 is 580-620° C., and the calcination time is 5-7 hours.

[0020] In some preferred embodiments, the calcination temperature in S5 is 800-1000° C., and the calcination time is 3-5 hours.

[0021] In some preferred embodiments, the zirconium nitrate and sodium tungstate are purchased from Sinopharm Chemical Reagent Co., Ltd. and are of analytical grade.

[0022] In some preferred embodiments, the method for preparing the nano-porous carbon is to calcine chopped waste straw at 600° C. to obtain the nano-porous carbon APC.

[0023] Beneficial Effects

[0024] 1. The present invention provides a catalyst for synthesizing acetonitrile and a preparation method thereof. The catalyst of the present invention uses nanoporous carbon (APC) as a carrier and zirconium-tungsten bimetallic as an active component, which can improve the yield of acetonitrile. The catalyst for synthesizing acetonitrile of the present invention can maintain high activity and selectivity for a long time, so that the yield can reach more than 99%, and the conversion rate can reach 99.99%. It can maintain high activity and selectivity for a long time, and can be revived for multiple uses, so that the service life is increased.

[0025] 2. The catalyst of the present invention uses nano-scale porous carbon as a carrier and supports the metal compound by an impregnation method, and the catalyst preparation method is simple.

[0026] 3. The nano-scale porous carbon used in the present invention is made from waste straw as raw material, which is a waste utilization and conforms to the production method of green chemical industry. DETAILED DESCRIPTION

[0027] Example 1

[0028] Example 1 provides a method for preparing a novel acetonitrile catalyst, comprising the following steps:

[0029] In a water bath equipped with a heating device and mechanical stirring, add 200 mL of deionized water and 10.4 g of zirconium nitrate pentahydrate to prepare an aqueous solution, then add 20.0 g of nanoporous carbon, stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 600°C for 6 hours to obtain 30% ZrO 2 Loading amount (based on the mass of nanoporous carbon) of ZrO 2 / APC; add 10g sodium tungstate to 150mL water to prepare an aqueous solution, add 20.0g ZrO 2 / APC; stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 900°C for 4 hours to obtain 30ZrO 2 / 35WO 3 / APC, ZrO 2 The loading is 30%, WO 3 The loading was 35%.

[0030] The above-mentioned zirconium-tungsten porous carbon catalyst is loaded into a reactor for acetic acid ammoniation and dehydration. The reactor is divided into a vaporization section and a reaction section. The reaction section is a fixed bed reactor, which is filled with a zirconium-tungsten porous carbon catalyst. After the acetic acid is vaporized, it is mixed with ammonia. The ammonia enters the vaporization mixing section at a rate of 300L / h. The acetic acid addition rate is controlled so that the two raw materials are mixed in a molar ratio of 1:1.3, preheated to 220°C, enter the raw material distributor, and then enter the bed layer containing the above-mentioned catalyst. The reaction temperature in the bed layer is 390°C; the top pressure of the reactor is 0.07KPa, and the retention time of the material in the reactor is 3s. The product obtained by the reaction is absorbed by 1000mL of water after condensation to obtain 1149g of absorption liquid.

[0031] The zirconium nitrate and sodium tungstate were purchased from Sinopharm Chemical Reagent Co., Ltd. and were of analytical grade.

[0032] The method for preparing the nano-scale porous carbon is to calcine chopped waste straw at 600° C. to obtain the nano-scale porous carbon APC.

[0033] Example 2

[0034] Example 2 provides a method for preparing a novel acetonitrile catalyst, comprising the following steps:

[0035] In a water bath equipped with a heating device and mechanical stirring, add 200 mL of deionized water and 14 g of zirconium nitrate pentahydrate to prepare an aqueous solution, then add 20.0 g of nanoporous carbon, stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 600°C for 6 hours to obtain 30% ZrO 2 Loading amount (based on the mass of nanoporous carbon) of ZrO 2 / APC; 12.5g sodium tungstate was added to 150mL water to prepare an aqueous solution, and 20.0g ZrO 2 / APC; stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 900°C for 4 hours to obtain 35ZrO 2 / 40WO 3 / APC, ZrO 2 The loading is 35%, WO 3 The loading is 40%.

[0036] The above-mentioned zirconium-tungsten porous carbon catalyst is loaded into a reactor for acetic acid ammoniation and dehydration. The reactor is divided into a vaporization section and a reaction section. The reaction section is a fixed bed reactor, and the zirconium-tungsten porous carbon catalyst is filled inside. 120g of acetic acid is vaporized and mixed with ammonia. The ammonia enters the vaporization mixing section at a rate of 300L / h. The acetic acid addition rate is controlled so that the two raw materials are mixed in a molar ratio of 1:1.3, preheated to 220°C, enter the raw material distributor, and then enter the bed layer containing the above-mentioned catalyst. The reaction temperature in the bed layer is 390°C; the top pressure of the reactor is 0.07KPa, and the retention time of the material in the reactor is 3s. The product obtained by the reaction is absorbed by 1000mL of water after condensation to obtain 1156g of absorption liquid.

[0037] The zirconium nitrate and sodium tungstate were purchased from Sinopharm Chemical Reagent Co., Ltd. and were of analytical grade.

[0038] The method for preparing the nano-scale porous carbon is to calcine chopped waste straw at 600° C. to obtain the nano-scale porous carbon APC.

[0039] Comparative Example 1

[0040] Comparative Example 1 provides a method for preparing a novel acetonitrile catalyst, comprising the following steps:

[0041] In a water bath equipped with a heating device and mechanical stirring, add 200 mL of deionized water and 10.4 g of zirconium nitrate pentahydrate to prepare an aqueous solution, then add 20.0 g of nanoporous carbon, stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 500°C for 6 hours to obtain 30% ZrO 2Loading amount (based on the mass of nanoporous carbon) of ZrO 2 / APC; add 10g sodium tungstate to 150mL water to prepare an aqueous solution, add 20.0g ZrO 2 / APC; stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 900°C for 4 hours to obtain 30ZrO 2 / 35WO 3 / APC, ZrO 2 The loading amount is 30%, WO 3 The loading was 35%.

[0042] The above-mentioned zirconium-tungsten porous carbon catalyst is loaded into a reactor for acetic acid ammoniation and dehydration. The reactor is divided into a vaporization section and a reaction section. The reaction section is a fixed bed reactor, which is filled with a zirconium-tungsten porous carbon catalyst. After the acetic acid is vaporized, it is mixed with ammonia. The ammonia enters the vaporization mixing section at a rate of 300L / h. The acetic acid addition rate is controlled so that the two raw materials are mixed in a molar ratio of 1:1.3, preheated to 220°C, enter the raw material distributor, and then enter the bed layer containing the above-mentioned catalyst. The reaction temperature in the bed layer is 390°C; the top pressure of the reactor is 0.07KPa, and the retention time of the material in the reactor is 3s. The product obtained by the reaction is absorbed by 1000mL of water after condensation to obtain 1174g of absorption liquid.

[0043] The zirconium nitrate and sodium tungstate were purchased from Sinopharm Chemical Reagent Co., Ltd. and were of analytical grade.

[0044] The method for preparing the nano-scale porous carbon is to calcine chopped waste straw at 600° C. to obtain the nano-scale porous carbon APC.

[0045] Comparative Example 2

[0046] Comparative Example 2 provides a method for preparing a novel acetonitrile catalyst, comprising the following steps:

[0047] In a water bath equipped with a heating device and mechanical stirring, add 200 ml of deionized water and 10.4 g of zirconium nitrate pentahydrate to prepare an aqueous solution, then add 20.0 g of nanoporous carbon, stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 700°C for 6 hours to obtain 30% ZrO 2 Loading amount (based on the mass of nanoporous carbon) of ZrO 2 / APC; add 10g sodium tungstate to 150mL water to prepare an aqueous solution, add 20.0g ZrO 2 / APC; stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 900°C for 4 hours to obtain 30ZrO2 / 35WO 3 / APC, ZrO 2 The loading is 30%, WO 3 The loading was 35%.

[0048] The above-mentioned zirconium-tungsten porous carbon catalyst is loaded into a reactor for acetic acid ammoniation and dehydration. The reactor is divided into a vaporization section and a reaction section. The reaction section is a fixed bed reactor, which is filled with a zirconium-tungsten porous carbon catalyst. After the acetic acid is vaporized, it is mixed with ammonia. The ammonia enters the vaporization mixing section at a rate of 300L / h. The acetic acid addition rate is controlled so that the two raw materials are mixed in a molar ratio of 1:1.3, preheated to 220°C, enter the raw material distributor, and then enter the bed layer containing the above-mentioned catalyst. The reaction temperature in the bed layer is 390°C; the top pressure of the reactor is 0.07KPa, and the retention time of the material in the reactor is 3s. The product obtained by the reaction is absorbed by 1000mL of water after condensation to obtain 1134g of absorption liquid.

[0049] The zirconium nitrate and sodium tungstate were purchased from Sinopharm Chemical Reagent Co., Ltd. and were of analytical grade.

[0050] The method for preparing the nano-scale porous carbon is to calcine chopped waste straw at 600° C. to obtain the nano-scale porous carbon APC.

[0051] Comparative Example 3

[0052] Comparative Example 3 provides a method for preparing a novel acetonitrile catalyst, comprising the following steps:

[0053] In a water bath equipped with a heating device and mechanical stirring, 200 mL of deionized water and 14 g of zirconium nitrate pentahydrate were added to prepare a zirconium nitrate aqueous solution, and then 20.0 g of MCM-41 (purchased from Shanghai Xinnian Petrochemical Additive Co., Ltd.) was added and stirred for 2 h. Then, the mixture was evaporated to dryness in a water bath at 85 ° C, dried at 120 ° C overnight, and calcined at 600 ° C for 6 h to obtain 35% ZrO 2 Loading amount (based on the mass of MCM-41) of ZrO 2 / MCM-41; 12.5g sodium tungstate was added into 150mL water to prepare sodium tungstate aqueous solution, and 20.0g ZrO 2 / MCM-41; stir and mix evenly for 2 hours, then evaporate to dryness in a water bath at 85°C, dry overnight at 120°C, and calcine at 900°C for 4 hours to obtain a zirconium-tungsten catalyst, 35ZrO 2 / 40WO 3 / MCM-41, ZrO 2 The loading is 35%, WO 3 The loading is 40%.

[0054] The above 35ZrO2 / 40WO 3 / MCM-41 is loaded into the reactor for acetic acid ammoniation dehydration. The reactor is divided into a vaporization section and a reaction section. The reaction section is a fixed bed reactor filled with 35ZrO 2 / 40WO 3 / MCM-41, acetic acid is vaporized and mixed with ammonia, ammonia enters the vaporization mixing section at a rate of 300L / h, the acetic acid addition rate is controlled to make the two raw material gases mixed at a molar ratio of 1:1.3, preheated to 220°C, enter the raw material distributor, and then enter the bed layer containing the above-mentioned catalyst, the reaction temperature in the bed layer is 390°C; the reactor top pressure is 0.07KPa, the material retention time in the reactor is 3s, the product obtained by the reaction is absorbed by 1000mL of water after condensation, and 1189g of absorption liquid is obtained.

[0055] The zirconium nitrate and sodium tungstate were purchased from Sinopharm Chemical Reagent Co., Ltd. and were of analytical grade.

[0056] Comparative Example 4

[0057] Comparative Example 4 provides a method for preparing a novel acetonitrile catalyst, comprising the following steps:

[0058] In a water bath equipped with a heating device and mechanical stirring, add 200 ml of deionized water and 10.4 g of zirconium nitrate pentahydrate to prepare an aqueous solution, then add 20.0 g of MCM-41 (purchased from Shanghai Xinnian Petrochemical Additive Co., Ltd.), stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 600°C for 6 hours to obtain 30% ZrO 2 Loading amount (based on the mass of MCM-41) of ZrO 2 / MCM-41; add 10g sodium tungstate to 150mL water to prepare an aqueous solution, add 20.0g ZrO 2 / MCM-41; stir and mix evenly for about 2 hours, then slowly stir and evaporate to dryness in a water bath at 85°C, dry at 120°C overnight, and calcine at 900°C for 4 hours to obtain 30ZrO 2 / 35WO 3 / MCM-41, ZrO 2 The loading is 30%, WO 3 The loading was 35%.

[0059] The above 30ZrO 2 / 35WO 3 / MCM-41 is loaded into the reactor for acetic acid ammoniation dehydration. The reactor is divided into a vaporization section and a reaction section. The reaction section is a fixed bed reactor filled with 30ZrO 2 / 35WO 3 / MCM-41, acetic acid is vaporized and mixed with ammonia, ammonia enters the vaporization mixing section at a rate of 300L / h, the acetic acid addition rate is controlled to make the two raw material gases mixed at a molar ratio of 1:1.3, preheated to 220°C, enter the raw material distributor, and then enter the bed layer containing the above-mentioned catalyst, the reaction temperature in the bed layer is 390°C; the pressure at the top of the reactor is 0.07KPa, the retention time of the material in the reactor is 3s, and the product obtained by the reaction is absorbed by 1000mL of water after condensation to obtain 1213g of absorption liquid.

[0060] The zirconium nitrate and sodium tungstate were purchased from Sinopharm Chemical Reagent Co., Ltd. and were of analytical grade.

[0061] Performance Testing

[0062] 1. Examples 1 and 2 and Comparative Examples 1 to 4 were analyzed and identified by gas chromatography, and the conversion rate of acetonitrile prepared by the catalyst-catalyzed ammoniation and dehydration of acetic acid, the content of acetonitrile in the absorption liquid and the yield were recorded in Table 1.

[0063] Table 1

[0064]

[0065]

[0066] 2. Record the number of reuses, service life, conversion rate of acetonitrile prepared by catalytic ammoniation and dehydration of acetic acid after 12 months and 6 months of continuous use of the zirconium-tungsten catalyst prepared in Example 2 and Comparative Example 3, and the content and yield of acetonitrile in the absorption liquid.

[0067] Number of times of reuse Service life Conversion rate, content, yield Example 2 3 times 12 months 99.99%、2.48%、99.1% Comparative Example 3 2 times 6 months 98.5%、1.69%、87.6%

Claims

1. Use of a catalyst to catalyze the ammoniation and dehydration of acetic acid to prepare acetonitrile, It is characterized in that The catalyst composition includes ZrO 2 and WO 3 and nanoporous carbon, nanoporous carbon is denoted as APC; The ZrO 2 The mass percentage of nano-porous carbon is 25-45%; The WO 3 Accounting for ZrO 2 and the mass percentage of nano-porous carbon is 30-50%; The preparation method of the catalyst comprises the following steps: S1: adding zirconium nitrate to deionized water to prepare a zirconium nitrate aqueous solution; S2: adding nano-porous carbon to the zirconium nitrate aqueous solution, stirring and mixing evenly to obtain a zirconium nitrate-porous carbon aqueous solution; S3: Stir the zirconium nitrate-porous carbon aqueous solution in a water bath at 70-100°C and evaporate to dryness, dry it at 100-140°C overnight, take it out after drying, and calcine it to obtain ZrO 2 / APC; S4: Add sodium tungstate into deionized water to prepare a sodium tungstate aqueous solution; S5: Add ZrO to the sodium tungstate aqueous solution 2 / APC, stir and mix evenly, then stir and evaporate to dryness in a water bath at 85°C, dry overnight at 100-140°C, take out after drying, and calcine to obtain ZrO 2 / WO 3 / APC; The zirconium nitrate in S1 is zirconium nitrate pentahydrate; The calcination temperature in S3 is 580-620° C., and the calcination time is 5-7 hours.

2. The use according to claim 1, It is characterized in that The WO 3 Accounting for ZrO 2 The mass percentage of nano-porous carbon is 35-45%.

3. The use according to claim 1, It is characterized in that The stirring time of S2 is 1.5 to 3 hours.

4. The use according to claim 1, It is characterized in that The calcination temperature in S5 is 800-1000° C., and the calcination time is 3-5 hours.